DIN 6935 Cold Bending of Flat Rolled Steel

Bending Angle α and Thickness s:

The bending angle a can have any value between 0° and 180°. The thickness ‘s’ decreases by approximately 20 % in the rounded portion (see Figure 1).

DIN 695 Bending r Radius bending angle α and thickness s

To obtain uniform bends on bending rails, it is recommended that only bending radii from the series below be selected. The values printed in bold are to be preferred.

r11.21.622.53456810121620252832364045506380100

These bending radii comply with the radii according to DIN 250.


Table 1 gives the minimum permissible bending radii to be chosen for given sheet thicknesses and materials and for the applicable bending machines. The indicated values apply for bending angles α ≤ 120°. For bending angles α> 120° the next higher value in the table shall be used, e.g. if sheets of S 275 JR according to DIN EN 10025-2 are to be bent transverse to the rolling direction, with a thickness s = 6 mm, the minimum permissible bending radius is r= 10 mm for α ≤ 120° and r = 12 mm for α> 120°.

Table 1 — Minimum permissible bending radius r (Dimensions in millimetres)

Minimum permissible bending radius r for thicknesses s
SteelgradesFor bending transverse or parallel to the rolling directionUp to 1Over 1 up to 1.5Over 1.5 up to 2.5Over 2.5
up to 3
Over 3 up to 4Over 4 up to 5Over 5
up to 6
Over 6
up to 7
Over 7
up to 8
Over 8
up to 10
Over 10
up to 12
Over 12
up to 14
Over 14
up to 16
Over 16
up to 18
Over 18 up to 20
S 235 JR
S 235 JO
s 235 J2
Transverse11.62.535681012162025283640
Parallel11.62.5368101216202528324045
S 275 JR
S 275 JO
s 275 J2
Transverse1.223458101216202528324045
Parallel1.2234610121620253236404550
S 355 JR
S 355 JO
s 355 J2
Transverse1.62.54568101216202532364550
Parallel1.62.545810121620253236405063

Table 2 — Permissible deviations for minimum bending radii r (Dimensions in millimetres)

Steel gradesPermissible deviations for minimum bending radii r for thicknesses s
Up to 3     Over 3 up to 8      Over 8 up to 20
S 235 JR
S 235 JO
S 235 J2
+0.5

0
+1

0
+1.5

0
S 275 JR
S 275 JO
S 275 J2
+0.8

0
+1.5

0
+2

0
S 355 JR
S 355 JO
S 355 J2
+1

0
+2

0
+3

0

Key to Materials:

Table 3 provides examples of materials for which suitability for cold bending, cold flanging and cold curling is guaranteed, taking into account the minimum permissible bending radii specified in Table 1.

Table 3 — Key to materials (examples)

Type of steelSteel grade with a minimum tensile strength a
Over 360 MPa up to 510 MPaOver 430  MPa up to 580 MPaOver 510 MPa up to 680 MPa
Hot-rolled products of structural steels according to DIN EN 10025-2S 235 JRS 275 JRs 355 J2
a For nominal thicknesses < 3 mm

Minimum Leg Length:

When mechanically bending sections of sheet metal, the leg length b is approximately 4.r (see Figure 2).

MINIMUM LEG LENGTH. DIN 695 Bending r Radius bending angle α and thickness s

Permissible Deviations for Angular Positions on Bending Sections:

Permissible deviations for angular positions. DIN 695 Bending r Radius bending angle α and thickness s

Values apply for a ratio up to r : s =4. For a larger (r : s) ratio, a larger deviation due to spring back is to be expected (see Figure 3).

Table 4 — Permissible deviations of angular positions (Dimensions in millimetres)

Leg lengths a and b
(where the shorter leg length is regarded as the nominal length)
Up to 30Over 30 up to 50Over 50 up to 80Over   80   up  to 120Over 120
Permissible deviations of bending angle α± 2°±1° 45′± 1° 30′± 1° 15′± 1°

Calculation of Developed Lengths:

Developed length=a+b+𝓋. Depending on the value of the bending angle, 𝓋 varies and represents a compensating value which, at an opening angle β of 0° up to 65° (calculated value 65° 24′ 30″), can be negative or positive, and at an opening angle over 65° can only be negative.
Developed lengths shall be rounded up to the nearest full millimetre.

Opening Angle β 0° up to 90°:

compensating value, Opening Angle β 0° up to 90°,DIN 695 Bending r Radius bending angle α and thickness s
compensating value notation, Opening Angle β 0° up to 90°,DIN 695 Bending r Radius bending angle α and thickness s

Opening Angle β 90° up to 165°:

Opening Angle β 90° up to 165°, formula, DIN 695 Bending r Radius bending angle α and thickness s
Opening Angle β 90° up to 165°, formula, DIN 695 Bending r Radius bending angle α and thickness s

Opening Angle β 165° up to 180°:

Compensating value 𝓋 =0

The values for 𝓋 are negligibly small in this case and sufficiently accurate for practical applications.

Opening Angle β 165° up to 180° notation, formula, DIN 695 Bending r Radius bending angle α and thickness s

Correction Factor k to Determine the Cut Lengths of Bent Workpieces

The correction factor k gives the deviation of the position of the neutral line s/2 and can be calculated as follows:

Correction Factor k to Determine the Cut Lengths of Bent Workpieces, k formula, DIN 695 Bending r Radius bending angle α and thickness s

or can be taken from the following graphical representation in Figure 7, which represents the equation.

For r : s > 5, Equation (3) is no longer valid so that k= 1 applies.

Graphical representation of correction factor k, DIN 695 Bending r Radius bending angle α and thickness s
Figure 7 — Graphical representation of correction factor

If only minimum requirements are set for the determination of cut lengths, rounded values as grouped together in Table 5 may be used for the correction factor k.

Table 5 — Correction factor k, rounded values

 Internal bending- radius r as a function of sheet thickness sRatio
r : s
Over 0.65
up to   1
Over 1
up to   1.5
Over 1.5
up to  2.4
Over 2.4
up to  3.8
Over 3.8
Correction factor k
(rounded values)
0.60.70.80.91.0

For any value for β, r and s, the corresponding compensating values 𝓋 can also be identified by the use of the correction factor k together with the graphical representations of factors in DIN 6935, Supplement 1.

For calculated compensating values 𝓋 for several opening and bending angles based on the above formula for correction factor k, see DIN 6935, Supplement 2.

Representation and Position of Bend Lines for Developments

The bend line indicates the middle of the bending radius and shall be represented by a thin continuous line. The position of the bend line results from the abutting leg lengths a and b, with half of the positive or negative compensating value 𝓋 taken into account (see Figure 8).

Representation and position of the bend line (notation). DIN 695 Bending r Radius bending angle α and thickness s
Figure 8 — Representation and position of the bend line (notation)

Developments shall only be explicitly drawn if the shape of the cut sheet is not unambiguously determined by dimensioning and indication of the bend line.

Dimensioning and Calculation of Developed Lengths (Examples)

EXAMPLE 1:

Material: S 235 JR

Developed Length DIN 6935 Example
Dimensions in millimetres

Sum of leg lengths= 50 + 200 + 80 = 330

β 90°, r= 6, s=4

compensating value, Opening Angle β 0° up to 90°,DIN 695 Bending r Radius bending angle α and thickness s

𝓋= 3.14 x(0.5)x ( 6+2 x 0.74)- 2×10= -8.26

β 90°, r= 20, s=4

𝓋= -13.44

𝓋total = -8.26-13.44= -21.7

Developed Length = 330-21.7= 308.3 ≈ 309

EXAMPLE 2:

Material: S 235 JR

Developed Length DIN 6935 Example
Dimensions in millimetres

Sum of leg lengths= 50 + 170 + 246+50 = 516

β 90°, r= 20, s=12 , 𝓋= -25,41

β 45°, r= 20, s=12 , 𝓋= -6.12

β 135°, r= 32, s=12 , 𝓋= -7.25

𝓋total = -25.41-6.12-7.25= -38.78

Developed Length = 516-38.78= 477.22 ≈ 478

Development and Marking of Bend Line Position (Example)

Material: S 355 J2
All dimensions in millimetres.

Sum of leg lengths= 45 + 50 + 32 = 127

β 45°, r= 10, s=5 , 𝓋= -1.72

β 135°, r= 10, s=5 , 𝓋= -3.00

𝓋total = -1.72-3.00= -4.72

Developed Length = 127-4.72= 122.28 ≈ 123

Position of Bend Lines:

For leg length = 45, β 45°, r= 10, s=5 , 𝓋= -1.72

45- 1.72÷2= 45- 0.86 = 44.14 ≈ 44

For leg length = 32, β 135°, r= 10, s=5 , 𝓋= -3.00

32-3.00÷2=32-1.5=30.5 ≈ 31

Position of bend lines, DIN 695 Bending r Radius bending angle α and thickness s
Position of bend lines