PARA 55% Glass and Mineral Filled Material Data Sheet

PARA 55% Glass and Mineral Filled (Polyarylamide) Material Data Sheet

PARA 55% Glass and Mineral Filled Overview

PARA 55% glass and mineral filled is a grade of polyarylamide (PARA), designated Polyarylamide (55% glass and mineral filled). This PARA 55% glass and mineral filled material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PARA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PARA parts in-house and inspects them before shipment.

PARA 55% Glass and Mineral Filled Designation

Polyarylamide (55% glass and mineral filled)
TradenamesIxef

PARA 55% Glass and Mineral Filled Typical uses

Automotive, furniture, small appliances, lawn mowers, power tools, electrical contactors and switches, electrical motor components, cell phones, faucet components.

PARA 55% Glass and Mineral Filled Composition detail

Polymer45  %
Glass (fiber)20–30%
Mineral (unspecified)25–35%

PARA 55% Glass and Mineral Filled Physical properties

Density1.74–1.78g/cm3

PARA 55% Glass and Mineral Filled Mechanical properties

Young’s modulus18.4–22.9GPa
Specific stiffness10.4–13MN.m/kg
Yield strength (elastic limit)99.4–124MPa
Tensile strength111–135MPa
Specific strength56.5–70.5kN.m/kg
Elongation0.932–1.34% strain
Elongation at yield0.784–1.49% strain
Compressive modulus19.6–21.7GPa
Compressive strength140–155MPa
Flexural modulus16.4–19.6GPa
Flexural strength (modulus of rupture)160–196MPa
Shear modulus7.44–7.82GPa
Shear strength66.3–81.1MPa
Bulk modulus22.1–24.4GPa
Poisson’s ratio0.35–0.352 
Shape factor12.4
Hardness – Vickers32–35HV
Hardness – Rockwell M160–177 
Hardness – Rockwell R160–177 
Hardness – Shore D93–97 
Elastic stored energy (springs)238–379kJ/m3
Fatigue strength at 10^7 cycles46.7–51.6MPa

PARA 55% Glass and Mineral Filled Impact & fracture properties

Fracture toughness5.64–6.23MPa.m0.5
Toughness (G)1.48–1.98kJ/m2
Impact strength, notched 23 °C2.95–5.72kJ/m2
Impact strength, unnotched 23 °C15.4–22.6kJ/m2

PARA 55% Glass and Mineral Filled Thermal properties

Melting point266–281°C
Glass temperature78–92.2°C
Heat deflection temperature 0.45MPa237–258°C
Heat deflection temperature 1.8MPa210–230°C
Vicat softening point77–90°C
Maximum service temperature185–198°C
Thermal conductivity0.616–0.663W/m.°C
Specific heat capacity1150–1180J/kg.°C
Thermal expansion coefficient17.6–18.5µstrain/°C
Thermal shock resistance258–351°C
Thermal distortion resistance0.034–0.0371MW/m

PARA 55% Glass and Mineral Filled Electrical properties

Electrical resistivity2e20–5e21µohm.cm
Electrical conductivity3.45e-20–8.62e-19%IACS
Dielectric constant (relative permittivity)4.22–5.95 
Dissipation factor (dielectric loss tangent)0.0301–0.0794 
Dielectric strength (dielectric breakdown)25.2–42.9MV/m
Comparative tracking index600  V

PARA 55% Glass and Mineral Filled Magnetic properties

Magnetic typeNon-magnetic

PARA 55% Glass and Mineral Filled Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3230–3610m/s
Mechanical loss coefficient (tan delta)0.00592–0.00655 

PARA 55% Glass and Mineral Filled Absorption & permeability

Water absorption @ 24 hrs0.14–0.24%
Water absorption @ sat2.6–3.5%
Humidity absorption @ sat1.4–1.8%

PARA 55% Glass and Mineral Filled Processing properties

Polymer injection moldingLimited use
Polymer extrusionAcceptable
Polymer thermoformingLimited use
Linear mold shrinkage0.1 – 0.45 %
Melt temperature266 – 281 °C
Mold temperature118 – 141 °C
Molding pressure range30 – 150 MPa

PARA 55% Glass and Mineral Filled Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsLimited use
Oils and fuelsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Good
FlammabilitySlow-burning