PARA 40-45% Mineral Filled Material Data Sheet

PARA 40-45% Mineral Filled (Polyarylamide) Material Data Sheet

PARA 40-45% Mineral Filled Overview

PARA 40-45% mineral filled is a grade of polyarylamide (PARA), designated Polyarylamide (40-45% mineral filled). This PARA 40-45% mineral filled material data sheet covers its designation and tradenames, composition, physical, mechanical, thermal, electrical and magnetic properties, and water absorption, processing properties and durability. Looking for PARA parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined PARA parts in-house and inspects them before shipment.

PARA 40-45% Mineral Filled Designation

Polyarylamide (40-45% mineral filled)
TradenamesIXEF

PARA 40-45% Mineral Filled Typical uses

Automotive, furniture, small appliances, lawn mowers, power tools, electrical contactors and switches, electrical motor components, cell phones, faucet components.

PARA 40-45% Mineral Filled Composition detail

Polymer55–60%
Mineral (unspecified)40–45%

PARA 40-45% Mineral Filled Physical properties

Density1.59–1.62g/cm3

PARA 40-45% Mineral Filled Mechanical properties

Young’s modulus15.1–18.8GPa
Specific stiffness9.41–11.7MN.m/kg
Yield strength (elastic limit)99.4–124MPa
Tensile strength111–135MPa
Specific strength61.9–77.3kN.m/kg
Elongation1.04–1.5% strain
Elongation at yield0.879–1.67% strain
Compressive modulus16.1–17.8GPa
Compressive strength140–155MPa
Flexural modulus12.1–14.5GPa
Flexural strength (modulus of rupture)160–196MPa
Shear modulus6.13–6.45GPa
Shear strength66.3–81.1MPa
Bulk modulus17.8–19.7GPa
Poisson’s ratio0.331–0.349 
Shape factor10.9
Hardness – Vickers32–35HV
Hardness – Rockwell M160–177 
Hardness – Rockwell R160–177 
Hardness – Shore D93–97 
Hardness – Shore A98–100 
Elastic stored energy (springs)290–461kJ/m3
Fatigue strength at 10^7 cycles46.7–51.6MPa

PARA 40-45% Mineral Filled Impact & fracture properties

Fracture toughness5.42–5.99MPa.m0.5
Toughness (G)1.67–2.22kJ/m2
Impact strength, notched 23 °C1.91–3.7kJ/m2
Impact strength, unnotched 23 °C23.8–35kJ/m2

PARA 40-45% Mineral Filled Thermal properties

Melting point269–291°C
Glass temperature78–92.2°C
Heat deflection temperature 0.45MPa166–218°C
Heat deflection temperature 1.8MPa143–192°C
Vicat softening point77–90°C
Maximum service temperature188–207°C
Thermal conductivity0.498–0.615W/m.°C
Specific heat capacity1240–1260J/kg.°C
Thermal expansion coefficient13.2–18.8µstrain/°C
Thermal shock resistance333–525°C
Thermal distortion resistance0.0287–0.0431MW/m

PARA 40-45% Mineral Filled Electrical properties

Electrical resistivity2e18–5e19µohm.cm
Electrical conductivity3.45e-18–8.62e-17%IACS
Dielectric constant (relative permittivity)3.79–5.34 
Dissipation factor (dielectric loss tangent)0.0108–0.0286 
Dielectric strength (dielectric breakdown)17.8–30.4MV/m
Comparative tracking index500–550V

PARA 40-45% Mineral Filled Magnetic properties

Magnetic typeNon-magnetic

PARA 40-45% Mineral Filled Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3060–3430m/s
Mechanical loss coefficient (tan delta)0.00689–0.00761 

PARA 40-45% Mineral Filled Absorption & permeability

Water absorption @ 24 hrs0.27–0.43%
Water absorption @ sat3.2–4.2%
Humidity absorption @ sat1.7–2.3%

PARA 40-45% Mineral Filled Processing properties

Polymer injection moldingLimited use
Polymer extrusionAcceptable
Polymer thermoformingLimited use
Linear mold shrinkage0.15 – 0.5 %
Melt temperature269 – 291 °C
Mold temperature122 – 138 °C
Molding pressure range30 – 150 MPa

PARA 40-45% Mineral Filled Durability

Water (fresh)Excellent
Water (salt)Acceptable
Weak acidsUnacceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsLimited use
Oils and fuelsAcceptable
Oxidation at 500CUnacceptable
UV radiation (sunlight)Good