AISI 4042 Oil Quenched & Tempered at 650°C Material Data Sheet

AISI 4042 Oil Quenched & Tempered at 650°C Material Data Sheet

AISI 4042 Oil Quenched & Tempered at 650°C Overview

AISI 4042 tempered 650°C is AISI 4042 low alloy steel (UNS G40420) in the oil quenched & tempered at 650°C condition. This AISI 4042 tempered 650°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 4042 conditions in our AISI 4042 yield, tensile and hardness comparison. Looking for AISI 4042 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 4042 steel parts in-house and inspects them before shipment.

AISI 4042 Oil Quenched & Tempered at 650°C Designation

AISI 4042
ConditionTempered at 650°C & oil quenched
UNS numberG40420
US nameSAE 4047, SAE 4042, ASTM 4047, ASTM 4042, ASTM 10V40 100, ~ASTM 4042

AISI 4042 Oil Quenched & Tempered at 650°C Typical uses

Heavy duty shafts, connecting rods, high tensile bolts

AISI 4042 Oil Quenched & Tempered at 650°C Composition detail

C (carbon)0.4–0.45%
Fe (iron)97.9–98.6%
Mn (manganese)0.7–0.9%
Mo (molybdenum)0.2–0.3%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 4042 Oil Quenched & Tempered at 650°C Physical properties

Density7.8–7.9g/cm3

AISI 4042 Oil Quenched & Tempered at 650°C Mechanical properties

Young’s modulus201–212GPa
Specific stiffness25.6–27MN.m/kg
Yield strength (elastic limit)620–760MPa
Tensile strength710–875MPa
Specific strength79–96.8kN.m/kg
Elongation22–34% strain
Compressive strength620–760MPa
Flexural modulus201–212GPa
Flexural strength (modulus of rupture)620–760MPa
Shear modulus77–83GPa
Bulk modulus155–173GPa
Poisson’s ratio0.285–0.295 
Shape factor36
Hardness – Vickers220–270HV
Elastic stored energy (springs)939–1390kJ/m3
Fatigue strength at 10^7 cycles336–390MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
291–450MPa

AISI 4042 Oil Quenched & Tempered at 650°C Impact & fracture properties

Fracture toughness48–79MPa.m0.5
Toughness (G)11.7–28.8kJ/m2

AISI 4042 Oil Quenched & Tempered at 650°C Thermal properties

Melting point1430–1500°C
Maximum service temperature610–640°C
Minimum service temperature-68–-43°C
Thermal conductivity47–54W/m.°C
Specific heat capacity440–480J/kg.°C
Thermal expansion coefficient11–13µstrain/°C
Thermal shock resistance244–317°C
Thermal distortion resistance3.79–4.69MW/m
Latent heat of fusion265–280kJ/kg

AISI 4042 Oil Quenched & Tempered at 650°C Electrical properties

Electrical resistivity15–25µohm.cm
Electrical conductivity6.9–11.5%IACS
Galvanic potential-0.51–-0.43V

AISI 4042 Oil Quenched & Tempered at 650°C Magnetic properties

Magnetic typeMagnetic

AISI 4042 Oil Quenched & Tempered at 650°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5060–5200m/s
Mechanical loss coefficient (tan delta)5.1e-4–6.4e-4 

AISI 4042 Oil Quenched & Tempered at 650°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed20.1 m/min
Weldability
Notes: Preheating and post weld heat treatments may be required
Poor
Carbon equivalency0.557 – 0.66

AISI 4042 Oil Quenched & Tempered at 650°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 4042 Oil Quenched & Tempered at 650°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 4042 Oil Quenched & Tempered at 650°C Notes

AISI 4042 Oil Quenched & Tempered at 650°C Other notes
Commonly used for applications which require good shock resistance;

AISI 4042 Oil Quenched & Tempered at 650°C Standards with similar compositions

Mexico: 4042 to NMX-B-203-SCFI, 4042 to NMX-B-300, 4042H to NMX-B-268, 4042H to NMX-B-300, 4047 to NMX-B-203-SCFI, 4047 to NMX-B-300, 4047H to NMX-B-268, 4047H to NMX-B-300
Pan America: 4042 to COPANT 514, 4047 to COPANT 514
Serbia and Montenegro: C.1534
UK: 2/2 to BS 3111/1
USA: 4042, 4042 to ASTM A29/A29M, 4042 to ASTM A322-91, 4042 to ASTM A331-95, 4042 to ASTM A519, 4042 to SAE J770, 4042H to ASTM A331-95, 4047 to ASTM A29/A29M, 4047 to ASTM A331-95, 4047 to ASTM A519, 4047 to SAE J404, 4047 to SAE J770, 4053, Grade 4 to ASTM A194/A194M, UNS G40420, UNS G40470, UNS H40420, UNS H40470, UNS K14510
Tradenames: CARILLOY CARBON MOLYBDENUM, CARILLOY CARBON-MOLYBDENUM