AISI 4042 Oil Quenched & Tempered at 540°C Material Data Sheet
AISI 4042 Oil Quenched & Tempered at 540°C Material Data Sheet
AISI 4042 Oil Quenched & Tempered at 540°C Overview
AISI 4042 tempered 540°C is AISI 4042 low alloy steel (UNS G40420) in the oil quenched & tempered at 540°C condition. This AISI 4042 tempered 540°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 4042 conditions in our AISI 4042 yield, tensile and hardness comparison. Looking for AISI 4042 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 4042 steel parts in-house and inspects them before shipment.
AISI 4042 Oil Quenched & Tempered at 540°C Designation
AISI 4042 Oil Quenched & Tempered at 540°C Thermal properties
Melting point
1430
–
1500
°C
Maximum service temperature
500
–
530
°C
Minimum service temperature
-68
–
-38
°C
Thermal conductivity
47
–
54
W/m.°C
Specific heat capacity
440
–
480
J/kg.°C
Thermal expansion coefficient
11
–
13
µstrain/°C
Thermal shock resistance
311
–
408
°C
Thermal distortion resistance
3.79
–
4.69
MW/m
Latent heat of fusion
265
–
280
kJ/kg
AISI 4042 Oil Quenched & Tempered at 540°C Electrical properties
Electrical resistivity
15
–
25
µohm.cm
Electrical conductivity
6.9
–
11.5
%IACS
Galvanic potential
-0.51
–
-0.43
V
AISI 4042 Oil Quenched & Tempered at 540°C Magnetic properties
Magnetic type
Magnetic
AISI 4042 Oil Quenched & Tempered at 540°C Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5060
–
5200
m/s
Mechanical loss coefficient (tan delta)
4e-4
–
5.1e-4
AISI 4042 Oil Quenched & Tempered at 540°C Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
15.8 m/min
Weldability Notes: Preheating and post weld heat treatments may be required
Poor
Carbon equivalency
0.557 – 0.66
AISI 4042 Oil Quenched & Tempered at 540°C Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
AISI 4042 Oil Quenched & Tempered at 540°C Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible
AISI 4042 Oil Quenched & Tempered at 540°C Notes
AISI 4042 Oil Quenched & Tempered at 540°C Other notes
Commonly used for applications which require good shock resistance;
AISI 4042 Oil Quenched & Tempered at 540°C Standards with similar compositions
Mexico: 4042 to NMX-B-203-SCFI, 4042 to NMX-B-300, 4042H to NMX-B-268, 4042H to NMX-B-300, 4047 to NMX-B-203-SCFI, 4047 to NMX-B-300, 4047H to NMX-B-268, 4047H to NMX-B-300
Pan America: 4042 to COPANT 514, 4047 to COPANT 514
Serbia and Montenegro: C.1534
UK: 2/2 to BS 3111/1
USA: 4042, 4042 to ASTM A29/A29M, 4042 to ASTM A322-91, 4042 to ASTM A331-95, 4042 to ASTM A519, 4042 to SAE J770, 4042H to ASTM A331-95, 4047 to ASTM A29/A29M, 4047 to ASTM A331-95, 4047 to ASTM A519, 4047 to SAE J404, 4047 to SAE J770, 4053, Grade 4 to ASTM A194/A194M, UNS G40420, UNS G40470, UNS H40420, UNS H40470, UNS K14510