AISI 4037 Oil Quenched & Tempered at 315°C Material Data Sheet

AISI 4037 Oil Quenched & Tempered at 315°C Material Data Sheet

AISI 4037 Oil Quenched & Tempered at 315°C Overview

AISI 4037 tempered 315°C is AISI 4037 low alloy steel (UNS G40370) in the oil quenched & tempered at 315°C condition. This AISI 4037 tempered 315°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 4037 conditions in our AISI 4037 yield, tensile and hardness comparison. Looking for AISI 4037 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 4037 steel parts in-house and inspects them before shipment.

AISI 4037 Oil Quenched & Tempered at 315°C Designation

AISI 4037
ConditionTempered at 315°C & oil quenched
UNS numberG40370
US nameSAE 4037, SAE 4032H, ASTM L7A, ASTM 4042H, ASTM 4037H, ASTM 4037, ASTM 4032H, ASTM 4032, ~SAE 4032

AISI 4037 Oil Quenched & Tempered at 315°C Typical uses

Heavy duty shafts, connecting rods, high tensile bolts

AISI 4037 Oil Quenched & Tempered at 315°C Composition detail

C (carbon)0.35–0.4%
Fe (iron)98–98.6%
Mn (manganese)0.7–0.9%
Mo (molybdenum)0.2–0.3%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 4037 Oil Quenched & Tempered at 315°C Physical properties

Density7.8–7.9g/cm3

AISI 4037 Oil Quenched & Tempered at 315°C Mechanical properties

Young’s modulus201–212GPa
Specific stiffness25.6–27MN.m/kg
Yield strength (elastic limit)685–845MPa
Tensile strength855–1050MPa
Specific strength87.2–108kN.m/kg
Elongation11–17% strain
Compressive strength685–845MPa
Flexural modulus201–212GPa
Flexural strength (modulus of rupture)685–845MPa
Shear modulus77–83GPa
Bulk modulus155–173GPa
Poisson’s ratio0.285–0.295 
Shape factor32
Hardness – Vickers270–330HV
Elastic stored energy (springs)1150–1710kJ/m3
Fatigue strength at 10^7 cycles383–442MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
335–505MPa

AISI 4037 Oil Quenched & Tempered at 315°C Impact & fracture properties

Fracture toughness50–83MPa.m0.5
Toughness (G)12.7–31.7kJ/m2

AISI 4037 Oil Quenched & Tempered at 315°C Thermal properties

Melting point1440–1510°C
Maximum service temperature275–305°C
Minimum service temperature-68–-43°C
Thermal conductivity48–53W/m.°C
Specific heat capacity440–480J/kg.°C
Thermal expansion coefficient11–13µstrain/°C
Thermal shock resistance270–352°C
Thermal distortion resistance3.83–4.64MW/m
Latent heat of fusion265–280kJ/kg

AISI 4037 Oil Quenched & Tempered at 315°C Electrical properties

Electrical resistivity15–25µohm.cm
Electrical conductivity6.9–11.5%IACS
Galvanic potential-0.51–-0.43V

AISI 4037 Oil Quenched & Tempered at 315°C Magnetic properties

Magnetic typeMagnetic

AISI 4037 Oil Quenched & Tempered at 315°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5060–5200m/s
Mechanical loss coefficient (tan delta)4.4e-4–5.5e-4 

AISI 4037 Oil Quenched & Tempered at 315°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed16.5 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.507 – 0.61

AISI 4037 Oil Quenched & Tempered at 315°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 4037 Oil Quenched & Tempered at 315°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 4037 Oil Quenched & Tempered at 315°C Notes

AISI 4037 Oil Quenched & Tempered at 315°C Other notes
Commonly used for applications which require good shock resistance;

AISI 4037 Oil Quenched & Tempered at 315°C Standards with similar compositions

Australia: 4037 to AS 1444, En16C to AS G18
International: 36Mo3E to ISO 4954
Mexico: 4032 to NMX-B-300, 4032H to NMX-B-268, 4032H to NMX-B-300, 4037 to NMX-B-203-SCFI, 4037 to NMX-B-300, 4037H to NMX-B-268, 4037H to NMX-B-300
Pan America: 4037 to COPANT 334
Serbia and Montenegro: C.1436
UK: 2/1 to BS 3111/1
USA: 4032, 4032 to ASTM A29/A29M, 4032H to ASTM A331-95, 4037 to ASTM A29/A29M, 4037 to ASTM A331-95, 4037 to ASTM A519, 4037 to SAE J404, 4037 to SAE J770, 4037H to ASTM A331-95, L71 to ASTM A320/A320M, L7A to ASTM A320/A320M, UNS G40320, UNS G40370, UNS H40320, UNS H40370
Tradenames: SHARON 4000 SERIES, WEST NO. 7 (DURACAST), WEST NO. 7A (DURACAST)