AISI 3140 normalized is AISI 3140 low alloy steel (UNS G31400, EN 40NiCr6) in the normalized condition. This AISI 3140 normalized material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 3140 conditions in our AISI 3140 yield, tensile and hardness comparison. Looking for AISI 3140 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 3140 steel parts in-house and inspects them before shipment.
AISI 3140 Normalized Designation
AISI 3140
Condition
Normalized
UNS number
G31400
US name
ASTM A519
EN name
40NiCr6, BS S148, 640M40, EN111
EN number
1.5711, 1.5710
AISI 3140 Normalized Typical uses
General construction, general mechanical engineering, automotive, tools, axles, gears, springs.
AISI 3140 Normalized Composition detail
C (carbon)
0.38
–
0.43
%
Cr (chromium)
0.55
–
0.75
%
Fe (iron)
96.1
–
97.1
%
Mn (manganese)
0.7
–
0.9
%
Ni (nickel)
1.1
–
1.4
%
P (phosphorus)
0
–
0.04
%
S (sulfur)
0
–
0.04
%
Si (silicon)
0.15
–
0.35
%
AISI 3140 Normalized Physical properties
Density
7.8
–
7.9
g/cm3
AISI 3140 Normalized Mechanical properties
Young’s modulus
201
–
212
GPa
Specific stiffness
25.6
–
27
MN.m/kg
Yield strength (elastic limit)
540
–
660
MPa
Tensile strength
800
–
985
MPa
Specific strength
68.8
–
84.1
kN.m/kg
Elongation
16
–
24
% strain
Compressive strength
540
–
660
MPa
Flexural modulus
201
–
212
GPa
Flexural strength (modulus of rupture)
540
–
660
MPa
Shear modulus
77
–
83
GPa
Bulk modulus
155
–
173
GPa
Poisson’s ratio
0.285
–
0.295
Shape factor
41
Hardness – Vickers
240
–
290
HV
Elastic stored energy (springs)
712
–
1050
kJ/m3
Fatigue strength at 10^7 cycles
366
–
424
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
318
–
487
MPa
AISI 3140 Normalized Impact & fracture properties
Fracture toughness
66
–
105
MPa.m0.5
Toughness (G)
22
–
51.1
kJ/m2
AISI 3140 Normalized Thermal properties
Melting point
1430
–
1500
°C
Maximum service temperature
613
–
650
°C
Minimum service temperature
-68
–
-43
°C
Thermal conductivity
45
–
55
W/m.°C
Specific heat capacity
440
–
520
J/kg.°C
Thermal expansion coefficient
10.5
–
12
µstrain/°C
Thermal shock resistance
228
–
291
°C
Thermal distortion resistance
3.94
–
4.99
MW/m
Latent heat of fusion
265
–
280
kJ/kg
AISI 3140 Normalized Electrical properties
Electrical resistivity
15
–
25
µohm.cm
Electrical conductivity
6.9
–
11.5
%IACS
Galvanic potential
-0.5
–
-0.42
V
AISI 3140 Normalized Magnetic properties
Magnetic type
Magnetic
AISI 3140 Normalized Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5060
–
5200
m/s
Mechanical loss coefficient (tan delta)
5.2e-4
–
6.4e-4
AISI 3140 Normalized Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
18.3 m/min
Weldability Notes: Preheating is required, post weld heat treatment may be required
Good
Carbon equivalency
0.68 – 0.823
AISI 3140 Normalized Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
AISI 3140 Normalized Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible
AISI 3140 Normalized Standards with similar compositions
China: 40CrNi to GB/T 17107, 40CrNi to GB/T 3077, 40CrNi to GB/T 3078
India: 35Ni1Cr60 to IS 4368, 35Ni5Cr2 to IS 11169/1, 35Ni5Cr2 to IS 13352, 35Ni5Cr2 to IS 1570/4, 35Ni5Cr2 to IS 3930, 35Ni5Cr2 to IS 4367, 35Ni5Cr2 to IS 9175/24, 46Ni5Cr2 to IS 3445
Japan: SNC 236 to JIS G4053
Romania: 40CrNi12 to STAS 791, 40CrNi12S to STAS 791, 40CrNi12X to STAS 791, 40CrNi12XS to STAS 791, 41CrNi12 to STAS 791
Russia: 40KHN to GOST 4543, 45KHN to GOST 4543, 45KHN to GOST 8479
South Korea: SNC 236 to KS D 3708
USA: 3135, 3140, 3140 to ASTM A519, 3145, G31400 to SAE J775, NV4 to SAE J775, UNS G31400, UNS K22033, X3140