How do the AISI 4130 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 4130 (UNS G41300, EN 30CrMo4) side by side for 8 conditions: Annealed, Air Melted, Normalized, Air Melted, Quenched & Tempered, Water Quenched & Tempered at 205°C, Water Quenched & Tempered at 315°C, Water Quenched & Tempered at 425°C, Water Quenched & Tempered at 540°C, Water Quenched & Tempered at 650°C. All values are taken from the individual AISI 4130 material data sheets linked below.
AISI 4130 Yield, Tensile and Hardness by Condition
| Condition | Yield strength (MPa) | Tensile strength (MPa) | Hardness (HV) | Elongation (%) |
|---|---|---|---|---|
| Annealed | 320–400 | 500–620 | 145–185 | 22–34 |
| Air Melted, Normalized | 483–534 | 621–686 | 183–223 | 5–18 |
| Air Melted, Quenched & Tempered | 690–1140 | 862–1240 | 420–515 | 8–12 |
| Water Quenched & Tempered at 205°C | 1320–1610 | 1450–1770 | 420–515 | 8–12 |
| Water Quenched & Tempered at 315°C | 1240–1520 | 1350–1650 | 390–480 | 8.5–13.5 |
| Water Quenched & Tempered at 425°C | 1070–1320 | 1150–1410 | 345–420 | 10–16 |
| Water Quenched & Tempered at 540°C | 820–1000 | 925–1140 | 285–355 | 13–21 |
| Water Quenched & Tempered at 650°C | 630–775 | 730–895 | 225–275 | 17–27 |
AISI 4130 Differences Compared with Annealed
The table below shows how much each condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength or hardness.
| Condition | Yield strength | Tensile strength | Hardness | Elongation |
|---|---|---|---|---|
| Air Melted, Normalized | +41% | +17% | +23% | -59% |
| Air Melted, Quenched & Tempered | +154% | +88% | +183% | -64% |
| Water Quenched & Tempered at 205°C | +307% | +188% | +183% | -64% |
| Water Quenched & Tempered at 315°C | +283% | +168% | +164% | -61% |
| Water Quenched & Tempered at 425°C | +232% | +129% | +132% | -54% |
| Water Quenched & Tempered at 540°C | +153% | +84% | +94% | -39% |
| Water Quenched & Tempered at 650°C | +95% | +45% | +52% | -21% |
AISI 4130 Strength and Hardness Charts
AISI 4130 Heat Treatment Key Points
The highest tensile strength is reached in the water quenched & tempered at 205°C condition (1450–1770 MPa). The softest condition is annealed (145–185 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 205°C to 650°C lowers hardness from 420–515 HV to 225–275 HV, trading strength for toughness and ductility.
AISI 4130 Material Data Sheets
AISI 4130 Annealed | AISI 4130 Air Melted, Normalized | AISI 4130 Air Melted, Quenched & Tempered | AISI 4130 Water Quenched & Tempered at 205°C | AISI 4130 Water Quenched & Tempered at 315°C | AISI 4130 Water Quenched & Tempered at 425°C | AISI 4130 Water Quenched & Tempered at 540°C | AISI 4130 Water Quenched & Tempered at 650°C | All AISI 4130 conditions
Looking for AISI 4130 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 4130 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.