AISI 4135 Air Melted, Quenched & Tempered Material Data Sheet
AISI 4135 Air Melted, Quenched & Tempered Overview
| AISI 4135 quenched tempered is AISI 4135 low alloy steel (UNS G41350, EN 34CrMo4) in the air melted, quenched & tempered condition. This AISI 4135 quenched tempered material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 4135 conditions in our AISI 4135 yield, tensile and hardness comparison. Looking for AISI 4135 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 4135 steel parts in-house and inspects them before shipment. |
AISI 4135 Air Melted, Quenched & Tempered Designation
| AISI 4135 | |
| Condition | Quenched & tempered |
| UNS number | G41350 |
| US name | SAE 4137, SAE 4135H, SAE 4135, SAE 17-22-A S, ASTM L7M, ASTM L7B, ASTM G41370, ASTM G55, ASTM F70, ASTM F65, ASTM B1, ASTM 4137, ASTM 4130H, ASTM 4130, ~SAE 4130, ~ASTM H 70, ~ASTM H65, ~ASTM H55, ~ASTM G41300, ~ASTM G70, ~ASTM G65, ~ASTM 4130 |
| EN name | ~34CrMo4 |
| EN number | ~1.7226, ~1.722 |
| ISO name | 34CrMoS4, 33CrAlMo5-4, ~34CrMo4 |
| GB (Chinese) name | ~ML35CrMo |
| JIS (Japanese) name | SCM430, SCM 3 |
AISI 4135 Air Melted, Quenched & Tempered Typical uses
| General construction, general mechanical engineering, automotive, pressure vessels, pipework |
AISI 4135 Air Melted, Quenched & Tempered Composition detail
| C (carbon) | 0.33 | – | 0.38 | % |
| Cr (chromium) | 0.8 | – | 1.1 | % |
| Fe (iron) | 96.9 | – | 97.9 | % |
| Mn (manganese) | 0.7 | – | 0.9 | % |
| Mo (molybdenum) | 0.15 | – | 0.25 | % |
| P (phosphorus) | 0 | – | 0.035 | % |
| S (sulfur) | 0 | – | 0.04 | % |
| Si (silicon) | 0.15 | – | 0.35 | % |
AISI 4135 Air Melted, Quenched & Tempered Physical properties
| Density | 7.79 | – | 7.87 | g/cm3 |
AISI 4135 Air Melted, Quenched & Tempered Mechanical properties
| Young’s modulus | 200 | – | 210 | GPa |
| Specific stiffness | 25.5 | – | 26.9 | MN.m/kg |
| Yield strength (elastic limit) | 690 | – | 1210 | MPa |
| Tensile strength | 862 | – | 1380 | MPa |
| Specific strength | 88.1 | – | 155 | kN.m/kg |
| Elongation | 6 | – | 12 | % strain |
| Compressive strength | 752 | – | 1250 | MPa |
| Flexural modulus | 200 | – | 210 | GPa |
| Flexural strength (modulus of rupture) | 690 | – | 1210 | MPa |
| Shear modulus | 76 | – | 79.9 | GPa |
| Bulk modulus | 185 | – | 195 | GPa |
| Poisson’s ratio | 0.32 | – | 0.333 | |
| Shape factor | 26 | |||
| Hardness – Vickers | 320 | – | 390 | HV |
| Hardness – Brinell | 290 | – | 350 | HB |
| Elastic stored energy (springs) | 1240 | – | 3380 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 248 | – | 801 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 228 | – | 873 | MPa |
AISI 4135 Air Melted, Quenched & Tempered Impact & fracture properties
| Fracture toughness | 80 | – | 135 | MPa.m0.5 |
| Toughness (G) | 32.9 | – | 84.2 | kJ/m2 |
AISI 4135 Air Melted, Quenched & Tempered Thermal properties
| Melting point | 1380 | – | 1530 | °C |
| Maximum service temperature | 470 | – | 524 | °C |
| Minimum service temperature | -73 | – | -13 | °C |
| Thermal conductivity | 42 | – | 45.5 | W/m.°C |
| Specific heat capacity | 461 | – | 480 | J/kg.°C |
| Thermal expansion coefficient | 12.4 | – | 13.1 | µstrain/°C |
| Thermal shock resistance | 264 | – | 466 | °C |
| Thermal distortion resistance | 3.28 | – | 3.6 | MW/m |
| Latent heat of fusion | 265 | – | 280 | kJ/kg |
AISI 4135 Air Melted, Quenched & Tempered Electrical properties
| Electrical resistivity | 15 | – | 35 | µohm.cm |
| Electrical conductivity | 4.93 | – | 11.5 | %IACS |
| Galvanic potential | -0.5 | – | -0.42 | V |
AISI 4135 Air Melted, Quenched & Tempered Magnetic properties
| Magnetic type | Magnetic |
AISI 4135 Air Melted, Quenched & Tempered Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5050 | – | 5180 | m/s |
| Mechanical loss coefficient (tan delta) | 2e-4 | – | 6e-4 | |
AISI 4135 Air Melted, Quenched & Tempered Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Excellent |
| Metal hot forming | Excellent |
| Metal press forming | Excellent |
| Metal deep drawing | Limited use |
| Machining speed | 13.7 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Good |
| Carbon equivalency | 0.637 – 0.8 |
AISI 4135 Air Melted, Quenched & Tempered Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) | Acceptable |
| Flammability | Non-flammable |
AISI 4135 Air Melted, Quenched & Tempered Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments | Slightly susceptible |
AISI 4135 Air Melted, Quenched & Tempered Notes
| AISI 4135 Air Melted, Quenched & Tempered Warning |
| Some rare heat treatments of certain alloys may produce values for mechanical properties outside the given ranges, e.g. AISI 9255. tempered at 205C |
AISI 4135 Air Melted, Quenched & Tempered Standards with similar compositions
| Argentina: IRAM 4133 to IAS, IRAM 4137 to IAS |
| Belgium: 34CrMo4 to NBN 253-02, 41CrMo4 to NBN 253-02 |
| Bulgaria: 35ChM to BDS 6354 |
| Finland: Co.35Cr1.1Mo0.20 to SFS 459 |
| France: 34CD4 to AFNOR NF A35-552, 34CD4 to AFNOR NF A35-556, 34CrMo4RR to AFNOR NF A36-102, 35CD4 to AFNOR NF A35-552, 35CD4 to AFNOR NF A35-553, 35CD4 to AFNOR NF A35-556, 38CD4 to AFNOR NF A35-552, 38CD4 to AFNOR NF A35-557 |
| Germany: 1.7220 to DIN 1652, 1.7220 to DIN EN 10083, 1.7226 to DIN 1652, 34CrMo4 to DIN EN 10083, 34CrMoS4 to DIN 1652, 35CrMo4 to DIN |
| Hungary: CMo3 to MSZ 61, CMo3E to MSZ 61, CMo3Z to MSZ 6251 |
| International: 34CrMo4 to ISO 683-1, 34CrMo4 to ISO 683-18, 34CrMo4E to ISO 4954, 34CrMoS4 to ISO 683-1, 34CrMoS4 to ISO 683-18, Type 2a to ISO 683-4, Type 2b to ISO 683-4 |
| Italy: 34CrMo4KB to UNI 7356, 35CrMo4 to UNI 6403, 35CrMo4 to UNI 7845, 35CrMo4KB to UNI 7356, 38CrMo4 to UNI 5333, 38CrMo4KB to UNI 7356 |
| Japan: SCM 3 to JIS G4105 |
| Mexico: 4135 to NMX-B-203-SCFI, 4135 to NMX-B-300, 4135H to NMX-B-268, 4135H to NMX-B-300, 4137 to NMX-B-203-SCFI, 4137 to NMX-B-300, 4137H to NMX-B-268, 4137H to NMX-B-300 |
| Norway: CrMoII to NS |
| Pan America: 4135 to COPANT 334, 4135 to COPANT 514, 4137 to COPANT 514 |
| Romania: 34MoCr11 to STAS 791, 34MoCr11S to STAS 791, 34MoCr11X to STAS 791, 34MoCr11XS to STAS 791, T34MoCr09 to STAS 1773 |
| Serbia and Montenegro: C.4731, C.4781, C.4783 |
| South Korea: SCM 435 H to KS D 3754 |
| Spain: 35CrMo4 to UNE 36012, 35CrMo4-1 to UNE 36012, 35CrMo4DF to UNE 36034, 38CrMo4 to UNE 36012, F.1250 to UNE 36012, F.1253 to UNE 36012, F.1254 to UNE 36034, F.1255 to UNE 36012 |
| Sweden: 2234 to SS 142234 |
| UK: 34CrMo4 to BS EN 10083-1, 34CrMo4 to BS EN 10132-3, 34CrMo4 to BS EN 10250-3, 34CrMo4 to BS EN 10297-1, 34CrMoS4 to BS EN 10083-1, 5/1 to BS 3111/1 |
| USA: 4135, 4135 to ASTM A29/A29M, 4135 to ASTM A519, 4135 to ASTM A829/A829M, 4135 to DoD-F-24669/1, 4135 to MIL-S-16974E, 4135 to MIL-S-18733A, 4135 to SAE J404, 4135 to SAE J770, 4137, 4137 to ASTM A29/A29M, 4137 to ASTM A331-95, 4137 to ASTM A519, 4137 to ASTM A829/A829M, 4137 to SAE J404, 4137 to SAE J770, G41350 to ASTM A1031, G41370 to ASTM A1031, Grade F Class 55 to ASTM A372/A372M, Grade F Class 65 to ASTM A372/A372M, Grade F Class 70 to ASTM A372/A372M, L72 to ASTM A320/A320M, L7B to ASTM A320/A320M, MIL-T-6735 to MIL-T-6735A, UNS G41350, UNS G41370, UNS H41350, UNS H41370, UNS K13548 |
| Tradenames: 35 CR MO 4, ABRASALLOY, ASCOMETAL 35CD4, BOHLER V330, DF 38 CR MO 4, DIRO-34 CRMO 4, FAGERSTA C 643, FORTUNA TCM04, HEVA-DF-100, KRUPP 2330, KRUPP 34 CRMOS 4, POMPEY KD 33, STEEL 34 CR MO 4, TKS 34CRMO4, WITTEN KV 32 COL |