AISI 4135 Normalized Material Data Sheet

AISI 4135 Normalized Material Data Sheet

AISI 4135 Normalized Overview

AISI 4135 normalized is AISI 4135 low alloy steel (UNS G41350, EN 34CrMo4) in the normalized condition. This AISI 4135 normalized material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 4135 conditions in our AISI 4135 yield, tensile and hardness comparison. Looking for AISI 4135 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 4135 steel parts in-house and inspects them before shipment.

AISI 4135 Normalized Designation

AISI 4135
ConditionNormalized
UNS numberG41350
US nameSAE 4137, SAE 4135H, SAE 4135, SAE 17-22-A S, ASTM L7M, ASTM L7B, ASTM G41370, ASTM G55, ASTM F70, ASTM F65, ASTM B1, ASTM 4137, ASTM 4130H, ASTM 4130, ~SAE 4130, ~ASTM H 70, ~ASTM H65, ~ASTM H55, ~ASTM G41300, ~ASTM G70, ~ASTM G65, ~ASTM 4130
EN name~34CrMo4
EN number~1.7226, ~1.722
ISO name34CrMoS4, 33CrAlMo5-4, ~34CrMo4
GB (Chinese) name~ML35CrMo
JIS (Japanese) nameSCM430, SCM 3

AISI 4135 Normalized Typical uses

General construction, general mechanical engineering, automotive, pressure vessels, pipework

AISI 4135 Normalized Composition detail

C (carbon)0.33–0.38%
Cr (chromium)0.8–1.1%
Fe (iron)96.9–97.9%
Mn (manganese)0.7–0.9%
Mo (molybdenum)0.15–0.25%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 4135 Normalized Physical properties

Density7.79–7.87g/cm3

AISI 4135 Normalized Mechanical properties

Young’s modulus200–210GPa
Specific stiffness25.5–26.9MN.m/kg
Yield strength (elastic limit)483–586MPa
Tensile strength621–690MPa
Specific strength61.7–74.8kN.m/kg
Elongation8–18% strain
Compressive strength483–614MPa
Flexural modulus200–210GPa
Flexural strength (modulus of rupture)483–586MPa
Shear modulus76–79.9GPa
Bulk modulus185–195GPa
Poisson’s ratio0.32–0.333 
Shape factor45
Hardness – Vickers200–240HV
Hardness – Brinell190–230HB
Elastic stored energy (springs)573–831kJ/m3
Fatigue strength at 10^7 cycles338–368MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
311–400MPa

AISI 4135 Normalized Impact & fracture properties

Fracture toughness90–110MPa.m0.5
Toughness (G)39.8–58.5kJ/m2

AISI 4135 Normalized Thermal properties

Melting point1260–1580°C
Maximum service temperature470–524°C
Minimum service temperature-73–-43°C
Thermal conductivity48–52W/m.°C
Specific heat capacity461–480J/kg.°C
Thermal expansion coefficient12.4–13.1µstrain/°C
Thermal shock resistance184–226°C
Thermal distortion resistance3.74–4.11MW/m
Latent heat of fusion284–326kJ/kg

AISI 4135 Normalized Electrical properties

Electrical resistivity20–24µohm.cm
Electrical conductivity7.18–8.62%IACS
Galvanic potential-0.5–-0.42V

AISI 4135 Normalized Magnetic properties

Magnetic typeMagnetic

AISI 4135 Normalized Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5050–5180m/s
Mechanical loss coefficient (tan delta)4e-4–9e-4 

AISI 4135 Normalized Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed23.5 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.637 – 0.8

AISI 4135 Normalized Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 4135 Normalized Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 4135 Normalized Notes

AISI 4135 Normalized Warning
Some rare heat treatments of certain alloys may produce values for mechanical properties outside the given ranges, e.g. AISI 9255. tempered at 205C

AISI 4135 Normalized Standards with similar compositions

Argentina: IRAM 4133 to IAS, IRAM 4137 to IAS
Belgium: 34CrMo4 to NBN 253-02, 41CrMo4 to NBN 253-02
Bulgaria: 35ChM to BDS 6354
Finland: Co.35Cr1.1Mo0.20 to SFS 459
France: 34CD4 to AFNOR NF A35-552, 34CD4 to AFNOR NF A35-556, 34CrMo4RR to AFNOR NF A36-102, 35CD4 to AFNOR NF A35-552, 35CD4 to AFNOR NF A35-553, 35CD4 to AFNOR NF A35-556, 38CD4 to AFNOR NF A35-552, 38CD4 to AFNOR NF A35-557
Germany: 1.7220 to DIN 1652, 1.7220 to DIN EN 10083, 1.7226 to DIN 1652, 34CrMo4 to DIN EN 10083, 34CrMoS4 to DIN 1652, 35CrMo4 to DIN
Hungary: CMo3 to MSZ 61, CMo3E to MSZ 61, CMo3Z to MSZ 6251
International: 34CrMo4 to ISO 683-1, 34CrMo4 to ISO 683-18, 34CrMo4E to ISO 4954, 34CrMoS4 to ISO 683-1, 34CrMoS4 to ISO 683-18, Type 2a to ISO 683-4, Type 2b to ISO 683-4
Italy: 34CrMo4KB to UNI 7356, 35CrMo4 to UNI 6403, 35CrMo4 to UNI 7845, 35CrMo4KB to UNI 7356, 38CrMo4 to UNI 5333, 38CrMo4KB to UNI 7356
Japan: SCM 3 to JIS G4105
Mexico: 4135 to NMX-B-203-SCFI, 4135 to NMX-B-300, 4135H to NMX-B-268, 4135H to NMX-B-300, 4137 to NMX-B-203-SCFI, 4137 to NMX-B-300, 4137H to NMX-B-268, 4137H to NMX-B-300
Norway: CrMoII to NS
Pan America: 4135 to COPANT 334, 4135 to COPANT 514, 4137 to COPANT 514
Romania: 34MoCr11 to STAS 791, 34MoCr11S to STAS 791, 34MoCr11X to STAS 791, 34MoCr11XS to STAS 791, T34MoCr09 to STAS 1773
Serbia and Montenegro: C.4731, C.4781, C.4783
South Korea: SCM 435 H to KS D 3754
Spain: 35CrMo4 to UNE 36012, 35CrMo4-1 to UNE 36012, 35CrMo4DF to UNE 36034, 38CrMo4 to UNE 36012, F.1250 to UNE 36012, F.1253 to UNE 36012, F.1254 to UNE 36034, F.1255 to UNE 36012
Sweden: 2234 to SS 142234
UK: 34CrMo4 to BS EN 10083-1, 34CrMo4 to BS EN 10132-3, 34CrMo4 to BS EN 10250-3, 34CrMo4 to BS EN 10297-1, 34CrMoS4 to BS EN 10083-1, 5/1 to BS 3111/1
USA: 4135, 4135 to ASTM A29/A29M, 4135 to ASTM A519, 4135 to ASTM A829/A829M, 4135 to DoD-F-24669/1, 4135 to MIL-S-16974E, 4135 to MIL-S-18733A, 4135 to SAE J404, 4135 to SAE J770, 4137, 4137 to ASTM A29/A29M, 4137 to ASTM A331-95, 4137 to ASTM A519, 4137 to ASTM A829/A829M, 4137 to SAE J404, 4137 to SAE J770, G41350 to ASTM A1031, G41370 to ASTM A1031, Grade F Class 55 to ASTM A372/A372M, Grade F Class 65 to ASTM A372/A372M, Grade F Class 70 to ASTM A372/A372M, L72 to ASTM A320/A320M, L7B to ASTM A320/A320M, MIL-T-6735 to MIL-T-6735A, UNS G41350, UNS G41370, UNS H41350, UNS H41370, UNS K13548
Tradenames: 35 CR MO 4, ABRASALLOY, ASCOMETAL 35CD4, BOHLER V330, DF 38 CR MO 4, DIRO-34 CRMO 4, FAGERSTA C 643, FORTUNA TCM04, HEVA-DF-100, KRUPP 2330, KRUPP 34 CRMOS 4, POMPEY KD 33, STEEL 34 CR MO 4, TKS 34CRMO4, WITTEN KV 32 COL