AISI 4130 Water Quenched & Tempered at 315°C Material Data Sheet
AISI 4130 Water Quenched & Tempered at 315°C Material Data Sheet
AISI 4130 Water Quenched & Tempered at 315°C Overview
AISI 4130 tempered 315°C is AISI 4130 low alloy steel (UNS G41300, EN 30CrMo4) in the water quenched & tempered at 315°C condition. This AISI 4130 tempered 315°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 4130 conditions in our AISI 4130 yield, tensile and hardness comparison. Looking for AISI 4130 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 4130 steel parts in-house and inspects them before shipment.
AISI 4130 Water Quenched & Tempered at 315°C Designation
AISI 4130 Water Quenched & Tempered at 315°C Typical uses
General construction, general mechanical engineering, automotive, tools, axles, gears, springs.
AISI 4130 Water Quenched & Tempered at 315°C Composition detail
C (carbon)
0.28
–
0.33
%
Cr (chromium)
0.8
–
1.1
%
Fe (iron)
97.3
–
98.2
%
Mn (manganese)
0.4
–
0.6
%
Mo (molybdenum)
0.15
–
0.25
%
P (phosphorus)
0
–
0.035
%
S (sulfur)
0
–
0.04
%
Si (silicon)
0.15
–
0.35
%
AISI 4130 Water Quenched & Tempered at 315°C Physical properties
Density
7.8
–
7.9
g/cm3
AISI 4130 Water Quenched & Tempered at 315°C Mechanical properties
Young’s modulus
201
–
216
GPa
Specific stiffness
25.6
–
27.5
MN.m/kg
Yield strength (elastic limit)
1240
–
1520
MPa
Tensile strength
1350
–
1650
MPa
Specific strength
158
–
194
kN.m/kg
Elongation
8.5
–
13.5
% strain
Compressive strength
1240
–
1520
MPa
Flexural modulus
201
–
216
GPa
Flexural strength (modulus of rupture)
1240
–
1520
MPa
Shear modulus
77
–
85
GPa
Bulk modulus
155
–
176
GPa
Poisson’s ratio
0.285
–
0.295
Shape factor
17
Hardness – Vickers
390
–
480
HV
Hardness – Brinell
369
–
452
HB
Elastic stored energy (springs)
3720
–
5510
kJ/m3
Fatigue strength at 10^7 cycles
526
–
608
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
460
–
696
MPa
AISI 4130 Water Quenched & Tempered at 315°C Impact & fracture properties
Fracture toughness
30
–
55
MPa.m0.5
Toughness (G)
4.63
–
13.5
kJ/m2
AISI 4130 Water Quenched & Tempered at 315°C Thermal properties
Melting point
1460
–
1510
°C
Maximum service temperature
275
–
305
°C
Minimum service temperature
-58
–
-28
°C
Thermal conductivity
42
–
48
W/m.°C
Specific heat capacity
460
–
500
J/kg.°C
Thermal expansion coefficient
11
–
13
µstrain/°C
Thermal shock resistance
482
–
630
°C
Thermal distortion resistance
3.38
–
4.17
MW/m
Latent heat of fusion
265
–
280
kJ/kg
AISI 4130 Water Quenched & Tempered at 315°C Electrical properties
Electrical resistivity
20
–
25
µohm.cm
Electrical conductivity
6.9
–
8.62
%IACS
Galvanic potential
-0.5
–
-0.42
V
AISI 4130 Water Quenched & Tempered at 315°C Magnetic properties
Magnetic type
Magnetic
AISI 4130 Water Quenched & Tempered at 315°C Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5060
–
5250
m/s
Mechanical loss coefficient (tan delta)
2.6e-4
–
3.3e-4
AISI 4130 Water Quenched & Tempered at 315°C Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
10.4 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency
0.537 – 0.7
AISI 4130 Water Quenched & Tempered at 315°C Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
AISI 4130 Water Quenched & Tempered at 315°C Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Susceptible
AISI 4130 Water Quenched & Tempered at 315°C Standards with similar compositions
Argentina: IRAM 4130 to IAS
Australia: 4130 to AS 1444, 4130H to AS 1444
Czech Republic: 15131 to CSN 415131
India: 30Cr4Mo2 to IS 1570/4, IS 963 to IS 963
Italy: 30CrMo4 to UNI 6403, 30CrMo4 to UNI 7845, 30CrMo4 to UNI 7874
Japan: SCM 1 to JIS G4105, STH 21 to JIS G3429, STKS1 to JIS G3441, STKS3 to JIS G3441
Mexico: 4130 to NMX-B-203-SCFI, 4130 to NMX-B-300, 4130H to NMX-B-268, 4130H to NMX-B-300
Pan America: 4130 to COPANT 334, 4130 to COPANT 514
Poland: 30HM to PN-H-84030/04, 30HMA to PN-H-84030/04
Romania: 25MoCr11 to STAS, 33MoCr11q to STAS 9382/4
UK: 30CrMo4 to BS EN 10297-1
USA: 4130, 4130 to ASTM A29/A29M, 4130 to ASTM A331-95, 4130 to ASTM A513, 4130 to ASTM A519, 4130 to ASTM A829/A829M, 4130 to ASTM A866, 4130 to DoD-F-24669/1, 4130 to SAE J404, 4130H to ASTM A331-95, 4130H to SAE J1975, G41300 to ASTM A1031, G41300 to ASTM A506, G41300 to ASTM A507, G41300 to MIL-S-46059, Grade 11 to ASTM A646-95, Grade 3 to ASTM A983/A983M, Grade E Class 55 to ASTM A372/A372M, Grade E Class 65 to ASTM A372/A372M, Grade E Class 70 to ASTM A372/A372M, MIL-T-6736 to MIL-T-6736B, UNS G41300, UNS H41300, UNS K13047, UNS K13147