AISI 4130 Air Melted, Quenched & Tempered Material Data Sheet
AISI 4130 Air Melted, Quenched & Tempered Material Data Sheet
AISI 4130 Air Melted, Quenched & Tempered Overview
AISI 4130 quenched tempered is AISI 4130 low alloy steel (UNS G41300, EN 30CrMo4) in the air melted, quenched & tempered condition. This AISI 4130 quenched tempered material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 4130 conditions in our AISI 4130 yield, tensile and hardness comparison. Looking for AISI 4130 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 4130 steel parts in-house and inspects them before shipment.
AISI 4130 Air Melted, Quenched & Tempered Designation
AISI 4130 Air Melted, Quenched & Tempered Thermal properties
Melting point
1460
–
1510
°C
Maximum service temperature
445
–
496
°C
Minimum service temperature
-53
–
-28
°C
Thermal conductivity
41.5
–
45
W/m.°C
Specific heat capacity
461
–
480
J/kg.°C
Thermal expansion coefficient
12.4
–
13.1
µstrain/°C
Thermal shock resistance
264
–
437
°C
Thermal distortion resistance
3.24
–
3.55
MW/m
Latent heat of fusion
265
–
280
kJ/kg
AISI 4130 Air Melted, Quenched & Tempered Electrical properties
Electrical resistivity
20
–
25
µohm.cm
Electrical conductivity
6.9
–
8.62
%IACS
Galvanic potential
-0.5
–
-0.42
V
AISI 4130 Air Melted, Quenched & Tempered Magnetic properties
Magnetic type
Magnetic
AISI 4130 Air Melted, Quenched & Tempered Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5050
–
5180
m/s
Mechanical loss coefficient (tan delta)
2e-4
–
6e-4
AISI 4130 Air Melted, Quenched & Tempered Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
11.6 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency
0.537 – 0.7
AISI 4130 Air Melted, Quenched & Tempered Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
AISI 4130 Air Melted, Quenched & Tempered Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible
AISI 4130 Air Melted, Quenched & Tempered Notes
AISI 4130 Air Melted, Quenched & Tempered Warning
Some rare heat treatments of certain alloys may produce values for mechanical properties outside the given ranges, e.g. AISI 9255. tempered at 205C
AISI 4130 Air Melted, Quenched & Tempered Standards with similar compositions
Argentina: IRAM 4130 to IAS
Australia: 4130 to AS 1444, 4130H to AS 1444
Czech Republic: 15131 to CSN 415131
India: 30Cr4Mo2 to IS 1570/4, IS 963 to IS 963
Italy: 30CrMo4 to UNI 6403, 30CrMo4 to UNI 7845, 30CrMo4 to UNI 7874
Japan: SCM 1 to JIS G4105, STH 21 to JIS G3429, STKS1 to JIS G3441, STKS3 to JIS G3441
Mexico: 4130 to NMX-B-203-SCFI, 4130 to NMX-B-300, 4130H to NMX-B-268, 4130H to NMX-B-300
Pan America: 4130 to COPANT 334, 4130 to COPANT 514
Poland: 30HM to PN-H-84030/04, 30HMA to PN-H-84030/04
Romania: 25MoCr11 to STAS, 33MoCr11q to STAS 9382/4
UK: 30CrMo4 to BS EN 10297-1
USA: 4130, 4130 to ASTM A29/A29M, 4130 to ASTM A331-95, 4130 to ASTM A513, 4130 to ASTM A519, 4130 to ASTM A829/A829M, 4130 to ASTM A866, 4130 to DoD-F-24669/1, 4130 to SAE J404, 4130H to ASTM A331-95, 4130H to SAE J1975, G41300 to ASTM A1031, G41300 to ASTM A506, G41300 to ASTM A507, G41300 to MIL-S-46059, Grade 11 to ASTM A646-95, Grade 3 to ASTM A983/A983M, Grade E Class 55 to ASTM A372/A372M, Grade E Class 65 to ASTM A372/A372M, Grade E Class 70 to ASTM A372/A372M, MIL-T-6736 to MIL-T-6736B, UNS G41300, UNS H41300, UNS K13047, UNS K13147