AISI 5046 Oil Quenched & Tempered at 425°C Material Data Sheet

AISI 5046 Oil Quenched & Tempered at 425°C Material Data Sheet

AISI 5046 Oil Quenched & Tempered at 425°C Overview

AISI 5046 tempered 425°C is AISI 5046 low alloy steel (UNS G50460) in the oil quenched & tempered at 425°C condition. This AISI 5046 tempered 425°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 5046 conditions in our AISI 5046 yield, tensile and hardness comparison. Looking for AISI 5046 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 5046 steel parts in-house and inspects them before shipment.

AISI 5046 Oil Quenched & Tempered at 425°C Designation

AISI 5046
ConditionTempered at 425°C & oil quenched
UNS numberG50460
US nameSAE 5046H, SAE 5046, ASTM G50460, ASTM 5046H, ~ASTM 5046

AISI 5046 Oil Quenched & Tempered at 425°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 5046 Oil Quenched & Tempered at 425°C Composition detail

C (carbon)0.43–0.5%
Cr (chromium)0.2–0.35%
Fe (iron)97.7–98.5%
Mn (manganese)0.75–1%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 5046 Oil Quenched & Tempered at 425°C Physical properties

Density7.8–7.9g/cm3

AISI 5046 Oil Quenched & Tempered at 425°C Mechanical properties

Young’s modulus201–212GPa
Specific stiffness25.6–27MN.m/kg
Yield strength (elastic limit)840–1020MPa
Tensile strength1020–1260MPa
Specific strength107–130kN.m/kg
Elongation10–16% strain
Compressive strength840–1020MPa
Flexural modulus201–212GPa
Flexural strength (modulus of rupture)840–1020MPa
Shear modulus77–83GPa
Bulk modulus155–173GPa
Poisson’s ratio0.285–0.295 
Shape factor26
Hardness – Vickers305–375HV
Elastic stored energy (springs)1720–2500kJ/m3
Fatigue strength at 10^7 cycles434–502MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
378–576MPa

AISI 5046 Oil Quenched & Tempered at 425°C Impact & fracture properties

Fracture toughness46–76MPa.m0.5
Toughness (G)10.8–26.6kJ/m2

AISI 5046 Oil Quenched & Tempered at 425°C Thermal properties

Melting point1420–1500°C
Maximum service temperature385–415°C
Minimum service temperature-63–-38°C
Thermal conductivity40–50W/m.°C
Specific heat capacity440–520J/kg.°C
Thermal expansion coefficient11–13µstrain/°C
Thermal shock resistance330–426°C
Thermal distortion resistance3.26–4.29MW/m
Latent heat of fusion265–280kJ/kg

AISI 5046 Oil Quenched & Tempered at 425°C Electrical properties

Electrical resistivity15–30µohm.cm
Electrical conductivity5.75–11.5%IACS
Galvanic potential-0.51–-0.43V

AISI 5046 Oil Quenched & Tempered at 425°C Magnetic properties

Magnetic typeMagnetic

AISI 5046 Oil Quenched & Tempered at 425°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5060–5200m/s
Mechanical loss coefficient (tan delta)3.7e-4–4.6e-4 

AISI 5046 Oil Quenched & Tempered at 425°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed14.3 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.595 – 0.737

AISI 5046 Oil Quenched & Tempered at 425°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 5046 Oil Quenched & Tempered at 425°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 5046 Oil Quenched & Tempered at 425°C Standards with similar compositions

Belgium: 46Cr2 to NBN 251
France: 42C2 to AFNOR NF A35-557
Hungary: MC to MSZ 1745
India: 50C6 to IS 14698
Italy: C40 to UNI 6923
Mexico: 5046 to NMX-B-300, 5046H to NMX-B-268, 5046H to NMX-B-300, 50B44 to NMX-B-300, 50B44H to NMX-B-268, 50B44H to NMX-B-300, 50B46 to NMX-B-300, 50B46H to NMX-B-268, 50B46H to NMX-B-300
Pan America: 5046 to COPANT 514
Russia: OsV to GOST 4728
USA: 5046, 5046 to ASTM A29/A29M, 5046 to ASTM A519, 5046 to SAE J770, 50B44 to ASTM A331-95, 50B44 to ASTM A519, 50B46 to ASTM A29/A29M, 50B46 to ASTM A331-95, 50B46 to ASTM A519, 50B46 to ASTM A752/A752M, G50460 to ASTM A1031, Grade 2 to ASTM A983/A983M, UNS G50460, UNS H50460
Tradenames: FIRTH-BROWN CR1T, KRUPP 46 CR 1, POMPEY D 42 K, POMPEY FF 42 H, POMPEY TR4M, POMPEY TR5, POMPEY TR5M, POMPEY TRJ