AISI 4320 Annealed Material Data Sheet

AISI 4320 Annealed Material Data Sheet

AISI 4320 Annealed Overview

AISI 4320 annealed is AISI 4320 low alloy steel (UNS G43200) in the annealed condition. This AISI 4320 annealed material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 4320 conditions in our AISI 4320 yield, tensile and hardness comparison. Looking for AISI 4320 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 4320 steel parts in-house and inspects them before shipment.

AISI 4320 Annealed Designation

AISI 4320
ConditionAnnealed
UNS numberG43200
US nameAMS 6294, ~SAE 4320, ~SAE 4320, ~ASTM 4320, ~ASTM G43200, ~ASTM 4320H, ~ASTM 4320
ISO name~E460 Quality DD
JIS (Japanese) name~ SNCM 420, ~SNCM420RCH, ~SNCM420H

AISI 4320 Annealed Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 4320 Annealed Composition detail

C (carbon)0.17–0.22%
Cr (chromium)0.4–0.6%
Fe (iron)95.8–97%
Mn (manganese)0.45–0.65%
Mo (molybdenum)0.2–0.3%
Ni (nickel)1.65–2%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 4320 Annealed Physical properties

Density7.8–7.9g/cm3

AISI 4320 Annealed Mechanical properties

Young’s modulus201–212GPa
Specific stiffness25.6–27MN.m/kg
Yield strength (elastic limit)380–470MPa
Tensile strength520–640MPa
Specific strength48.4–59.9kN.m/kg
Elongation23–35% strain
Compressive strength550–670MPa
Flexural modulus201–212GPa
Flexural strength (modulus of rupture)550–670MPa
Shear modulus77–83GPa
Bulk modulus155–173GPa
Poisson’s ratio0.285–0.295 
Shape factor52
Hardness – Vickers150–190HV
Elastic stored energy (springs)353–530kJ/m3
Fatigue strength at 10^7 cycles270–314MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
234–362MPa

AISI 4320 Annealed Impact & fracture properties

Fracture toughness65–103MPa.m0.5
Toughness (G)21.4–49.2kJ/m2

AISI 4320 Annealed Thermal properties

Melting point1480–1520°C
Maximum service temperature639–661°C
Minimum service temperature-73–-48°C
Thermal conductivity35–50W/m.°C
Specific heat capacity440–520J/kg.°C
Thermal expansion coefficient10.5–12µstrain/°C
Thermal shock resistance161–207°C
Thermal distortion resistance3.09–4.5MW/m
Latent heat of fusion265–280kJ/kg

AISI 4320 Annealed Electrical properties

Electrical resistivity18–27µohm.cm
Electrical conductivity6.39–9.58%IACS
Galvanic potential-0.5–-0.42V

AISI 4320 Annealed Magnetic properties

Magnetic typeMagnetic

AISI 4320 Annealed Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5060–5200m/s
Mechanical loss coefficient (tan delta)7.6e-4–9.5e-4 

AISI 4320 Annealed Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed28.3 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.475 – 0.642

AISI 4320 Annealed Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 4320 Annealed Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 4320 Annealed Standards with similar compositions

Argentina: IRAM 4320 to IAS
China: 20CrNi2MoH to GB/T 5216, G20CrNi2Mo to GB 3203
France: 20NCD7 to AFNOR NF A35-565, 20NiCrMo7 to AFNOR NF A35-565
India: 20Ni7Cr2Mo2 to IS 1570/4, 20Ni7CrMo2 to IS 9175/30
International: 20NiCrMo7 to ISO 683-17
Italy: 18NiCrMo7 to UNI 7846, 18NiCrMo7 to UNI 8550, 20NiCrMo7 to UNI 3097
Japan: SNCM 420 to JIS G4053, SNCM23 to JIS G4103, SNCM420 to JIS G4103, SNCM420H to JIS G4052, SNCM420HRCH to JIS G3509-1, SNCM420RCH to JIS G3509-1
Mexico: 4320 to NMX-B-300, 4320H to NMX-B-268, 4320H to NMX-B-300
Pan America: 4320 to COPANT 334
Russia: 20KHN2M to GOST 4543
South Korea: SNCM 420 H to KS D 3754, SNCM 420 to KS D 3709
Spain: 20NiCrMo6 to UNE 36013, 20NiCrMo6-1 to UNE 36013, 20NiCrMo7 to UNE 36027, F.1525 to UNE 36013, F.1529 to UNE 36027, F.1535 to UNE 36013
UK: 20NiCrMo7 to BS EN ISO 683-17
USA: 4317, 4320, 4320 to ASTM A29/A29M, 4320 to ASTM A322-91, 4320 to ASTM A331-95, 4320 to ASTM A519, 4320 to ASTM A752/A752M, 4320 to SAE J404, 4320H, 4320H to ASTM A304, 4320H to ASTM A331-95, 4320H to ASTM A534, 4320H to SAE J1268, 4320H to SAE J1975, 4320RH to ASTM A914/A914M-92, 4320RH to SAE J1868, B29 to ASTM A534, G43200 to ASTM A1031, G43200 to ASTM A837/A837M, UNS G43200, UNS H43200
Tradenames: ACENOR F-1525, VM-20