AISI 4150 Oil Quenched & Tempered at 650°C Material Data Sheet
AISI 4150 Oil Quenched & Tempered at 650°C Overview
| AISI 4150 tempered 650°C is AISI 4150 low alloy steel (UNS G41500) in the oil quenched & tempered at 650°C condition. This AISI 4150 tempered 650°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 4150 conditions in our AISI 4150 yield, tensile and hardness comparison. Looking for AISI 4150 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 4150 steel parts in-house and inspects them before shipment. |
AISI 4150 Oil Quenched & Tempered at 650°C Designation
| AISI 4150 | |
| Condition | Tempered at 650°C & oil quenched |
| UNS number | G41500 |
| US name | SAE 4150, ASTM 4150, ASTM G41500, ASTM 1A 1, ASTM 4150H, ~SAE PS 40, ~SAE 4150H |
| GB (Chinese) name | 50CrMo |
AISI 4150 Oil Quenched & Tempered at 650°C Typical uses
| General construction, general mechanical engineering, automotive, tools, axles, gears, springs. |
AISI 4150 Oil Quenched & Tempered at 650°C Composition detail
| C (carbon) | 0.48 | – | 0.53 | % |
| Cr (chromium) | 0.8 | – | 1.1 | % |
| Fe (iron) | 96.7 | – | 97.7 | % |
| Mn (manganese) | 0.75 | – | 1 | % |
| Mo (molybdenum) | 0.15 | – | 0.25 | % |
| P (phosphorus) | 0 | – | 0.035 | % |
| S (sulfur) | 0 | – | 0.04 | % |
| Si (silicon) | 0.15 | – | 0.35 | % |
AISI 4150 Oil Quenched & Tempered at 650°C Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 4150 Oil Quenched & Tempered at 650°C Mechanical properties
| Young’s modulus | 201 | – | 212 | GPa |
| Specific stiffness | 25.6 | – | 27 | MN.m/kg |
| Yield strength (elastic limit) | 755 | – | 925 | MPa |
| Tensile strength | 860 | – | 1060 | MPa |
| Specific strength | 96.2 | – | 118 | kN.m/kg |
| Elongation | 15 | – | 23 | % strain |
| Compressive strength | 755 | – | 925 | MPa |
| Flexural modulus | 201 | – | 212 | GPa |
| Flexural strength (modulus of rupture) | 755 | – | 925 | MPa |
| Shear modulus | 77 | – | 83 | GPa |
| Bulk modulus | 155 | – | 173 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 29 | |||
| Hardness – Vickers | 265 | – | 325 | HV |
| Elastic stored energy (springs) | 1390 | – | 2060 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 385 | – | 445 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 336 | – | 510 | MPa |
AISI 4150 Oil Quenched & Tempered at 650°C Impact & fracture properties
| Fracture toughness | 45 | – | 74 | MPa.m0.5 |
| Toughness (G) | 10.3 | – | 25.3 | kJ/m2 |
AISI 4150 Oil Quenched & Tempered at 650°C Thermal properties
| Melting point | 1410 | – | 1500 | °C |
| Maximum service temperature | 601 | – | 640 | °C |
| Minimum service temperature | -68 | – | -38 | °C |
| Thermal conductivity | 40 | – | 46 | W/m.°C |
| Specific heat capacity | 450 | – | 490 | J/kg.°C |
| Thermal expansion coefficient | 11 | – | 13 | µstrain/°C |
| Thermal shock resistance | 297 | – | 386 | °C |
| Thermal distortion resistance | 3.22 | – | 3.99 | MW/m |
| Latent heat of fusion | 265 | – | 280 | kJ/kg |
AISI 4150 Oil Quenched & Tempered at 650°C Electrical properties
| Electrical resistivity | 20 | – | 25 | µohm.cm |
| Electrical conductivity | 6.9 | – | 8.62 | %IACS |
| Galvanic potential | -0.5 | – | -0.42 | V |
AISI 4150 Oil Quenched & Tempered at 650°C Magnetic properties
| Magnetic type | Magnetic |
AISI 4150 Oil Quenched & Tempered at 650°C Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5060 | – | 5200 | m/s |
| Mechanical loss coefficient (tan delta) | 4.2e-4 | – | 5.3e-4 | |
AISI 4150 Oil Quenched & Tempered at 650°C Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Excellent |
| Metal hot forming | Excellent |
| Metal press forming | Excellent |
| Metal deep drawing | Limited use |
| Machining speed | 16.5 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Good |
| Carbon equivalency | 0.795 – 0.967 |
AISI 4150 Oil Quenched & Tempered at 650°C Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) | Acceptable |
| Flammability | Non-flammable |
AISI 4150 Oil Quenched & Tempered at 650°C Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments | Slightly susceptible |
AISI 4150 Oil Quenched & Tempered at 650°C Standards with similar compositions
| Argentina: IRAM 4150 to IAS |
| Australia: 4150 to AS 1444, 4150H to AS 1444 |
| Germany: 1.3565 to DIN 17230, 1.7228 to DIN 1652, 1.7228 to DIN 17201, 1.7238 to DIN 17212, 48CrMo4 to DIN 17230, 49CrMo4 to DIN 17212, 50CrMo4 to DIN 1652, 50CrMo4 to DIN EN 10083 |
| International: 50CrMo4 to ISO 683-1, 50CrMo4 to ISO 683-18 |
| Japan: SCM 5 to JIS G4105, SCM5H to JIS G4052 |
| Mexico: 4145 to NMX-B-300, 4145H to NMX-B-268, 4145H to NMX-B-300, 4147 to NMX-B-203-SCFI, 4147 to NMX-B-300, 4147H to NMX-B-268, 4147H to NMX-B-300, 4150 to NMX-B-203-SCFI, 4150 to NMX-B-300, 4150H to NMX-B-268, 4150H to NMX-B-300 |
| Pan America: 4145 to COPANT 514, 4147 to COPANT 514, 4150 to COPANT 334, 4150 to COPANT 514 |
| Serbia and Montenegro: C.4733 |
| South Korea: SCM 445 H to KS D 3754 |
| Turkey: 51CrMoV4-17701 to TS 2288 |
| UK: 50CrMo4 to BS EN 10083-1, 50CrMo4 to BS EN 10250-3 |
| USA: 4145 to ASTM A29/A29M, 4145 to ASTM A331-95, 4145 to ASTM A519, 4145 to ASTM A829/A829M, 4145 to MIL-S-16974E, 4145 to SAE J404, 4145 to SAE J770, 4147 to ASTM A29/A29M, 4147 to ASTM A331-95, 4147 to ASTM A519, 4147 to SAE J770, 4147H to ASTM A331-95, 4150, 4150 to ASTM A29/A29M, 4150 to ASTM A331-95, 4150 to ASTM A519, 4150 to ASTM A829/A829M, 4150 to ASTM A866, 4150 to SAE J404, 4150H to ASTM A331-95, Class 1A Grade 1 to ASTM A649/A649M-99, Class 1A Grade 2 to ASTM A649/A649M-99, G41450 to ASTM A1031, G41470 to ASTM A1031, G41500 to ASTM A1031, Mn-Cr-Mo to MIL-B-12504E, ORD 4150 to MIL-B-11595E, PS 67, PS 67 to SAE J1081, UNS G41450, UNS G41470, UNS G41500, UNS H41450, UNS H41470, UNS H41500, UNS K15747 |
| Tradenames: DICA (FLAME HARD) CAST TO SHAPE, DIRO-49 CRMO 4, DIRO-50 CRMO 4, E 7228, KRUPP 49 CRMO 4, MTD 4, OVAKO 528, ROLEY ZCMO10, SHARON 4100 SERIES B, STEEL 50 CR MO 4, TKS 50CRMO4 |