AISI 4150 Oil Quenched & Tempered at 205°C Material Data Sheet

AISI 4150 Oil Quenched & Tempered at 205°C Material Data Sheet

AISI 4150 Oil Quenched & Tempered at 205°C Overview

AISI 4150 tempered 205°C is AISI 4150 low alloy steel (UNS G41500) in the oil quenched & tempered at 205°C condition. This AISI 4150 tempered 205°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 4150 conditions in our AISI 4150 yield, tensile and hardness comparison. Looking for AISI 4150 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 4150 steel parts in-house and inspects them before shipment.

AISI 4150 Oil Quenched & Tempered at 205°C Designation

AISI 4150
ConditionTempered at 205°C & oil quenched
UNS numberG41500
US nameSAE 4150, ASTM 4150, ASTM G41500, ASTM 1A 1, ASTM 4150H, ~SAE PS 40, ~SAE 4150H
GB (Chinese) name50CrMo

AISI 4150 Oil Quenched & Tempered at 205°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 4150 Oil Quenched & Tempered at 205°C Composition detail

C (carbon)0.48–0.53%
Cr (chromium)0.8–1.1%
Fe (iron)96.7–97.7%
Mn (manganese)0.75–1%
Mo (molybdenum)0.15–0.25%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 4150 Oil Quenched & Tempered at 205°C Physical properties

Density7.8–7.9g/cm3

AISI 4150 Oil Quenched & Tempered at 205°C Mechanical properties

Young’s modulus201–212GPa
Specific stiffness25.6–27MN.m/kg
Yield strength (elastic limit)1550–1900MPa
Tensile strength1740–2120MPa
Specific strength197–242kN.m/kg
Elongation8–12% strain
Compressive strength1550–1900MPa
Flexural modulus201–212GPa
Flexural strength (modulus of rupture)1550–1900MPa
Shear modulus77–83GPa
Bulk modulus155–173GPa
Poisson’s ratio0.285–0.295 
Shape factor13
Hardness – Vickers475–585HV
Elastic stored energy (springs)5870–8670kJ/m3
Fatigue strength at 10^7 cycles630–725MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
553–826MPa

AISI 4150 Oil Quenched & Tempered at 205°C Impact & fracture properties

Fracture toughness23–47MPa.m0.5
Toughness (G)2.82–9.74kJ/m2

AISI 4150 Oil Quenched & Tempered at 205°C Thermal properties

Melting point1410–1500°C
Maximum service temperature165–195°C
Minimum service temperature-48–-18°C
Thermal conductivity40–46W/m.°C
Specific heat capacity450–490J/kg.°C
Thermal expansion coefficient11–13µstrain/°C
Thermal shock resistance609–793°C
Thermal distortion resistance3.22–3.99MW/m
Latent heat of fusion265–280kJ/kg

AISI 4150 Oil Quenched & Tempered at 205°C Electrical properties

Electrical resistivity20–25µohm.cm
Electrical conductivity6.9–8.62%IACS
Galvanic potential-0.5–-0.42V

AISI 4150 Oil Quenched & Tempered at 205°C Magnetic properties

Magnetic typeMagnetic

AISI 4150 Oil Quenched & Tempered at 205°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5060–5200m/s
Mechanical loss coefficient (tan delta)2e-4–2.6e-4 

AISI 4150 Oil Quenched & Tempered at 205°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed8.23 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.795 – 0.967

AISI 4150 Oil Quenched & Tempered at 205°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 4150 Oil Quenched & Tempered at 205°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Susceptible

AISI 4150 Oil Quenched & Tempered at 205°C Standards with similar compositions

Argentina: IRAM 4150 to IAS
Australia: 4150 to AS 1444, 4150H to AS 1444
Germany: 1.3565 to DIN 17230, 1.7228 to DIN 1652, 1.7228 to DIN 17201, 1.7238 to DIN 17212, 48CrMo4 to DIN 17230, 49CrMo4 to DIN 17212, 50CrMo4 to DIN 1652, 50CrMo4 to DIN EN 10083
International: 50CrMo4 to ISO 683-1, 50CrMo4 to ISO 683-18
Japan: SCM 5 to JIS G4105, SCM5H to JIS G4052
Mexico: 4145 to NMX-B-300, 4145H to NMX-B-268, 4145H to NMX-B-300, 4147 to NMX-B-203-SCFI, 4147 to NMX-B-300, 4147H to NMX-B-268, 4147H to NMX-B-300, 4150 to NMX-B-203-SCFI, 4150 to NMX-B-300, 4150H to NMX-B-268, 4150H to NMX-B-300
Pan America: 4145 to COPANT 514, 4147 to COPANT 514, 4150 to COPANT 334, 4150 to COPANT 514
Serbia and Montenegro: C.4733
South Korea: SCM 445 H to KS D 3754
Turkey: 51CrMoV4-17701 to TS 2288
UK: 50CrMo4 to BS EN 10083-1, 50CrMo4 to BS EN 10250-3
USA: 4145 to ASTM A29/A29M, 4145 to ASTM A331-95, 4145 to ASTM A519, 4145 to ASTM A829/A829M, 4145 to MIL-S-16974E, 4145 to SAE J404, 4145 to SAE J770, 4147 to ASTM A29/A29M, 4147 to ASTM A331-95, 4147 to ASTM A519, 4147 to SAE J770, 4147H to ASTM A331-95, 4150, 4150 to ASTM A29/A29M, 4150 to ASTM A331-95, 4150 to ASTM A519, 4150 to ASTM A829/A829M, 4150 to ASTM A866, 4150 to SAE J404, 4150H to ASTM A331-95, Class 1A Grade 1 to ASTM A649/A649M-99, Class 1A Grade 2 to ASTM A649/A649M-99, G41450 to ASTM A1031, G41470 to ASTM A1031, G41500 to ASTM A1031, Mn-Cr-Mo to MIL-B-12504E, ORD 4150 to MIL-B-11595E, PS 67, PS 67 to SAE J1081, UNS G41450, UNS G41470, UNS G41500, UNS H41450, UNS H41470, UNS H41500, UNS K15747
Tradenames: DICA (FLAME HARD) CAST TO SHAPE, DIRO-49 CRMO 4, DIRO-50 CRMO 4, E 7228, KRUPP 49 CRMO 4, MTD 4, OVAKO 528, ROLEY ZCMO10, SHARON 4100 SERIES B, STEEL 50 CR MO 4, TKS 50CRMO4