AISI 4140 Oil Quenched & Tempered at 650°C Material Data Sheet
AISI 4140 Oil Quenched & Tempered at 650°C Overview
| AISI 4140 tempered 650°C is AISI 4140 low alloy steel (UNS G41400, EN 42CrMo4) in the oil quenched & tempered at 650°C condition. This AISI 4140 tempered 650°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 4140 conditions in our AISI 4140 yield, tensile and hardness comparison. Looking for AISI 4140 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 4140 steel parts in-house and inspects them before shipment. |
AISI 4140 Oil Quenched & Tempered at 650°C Designation
| AISI 4140 | |
| Condition | Tempered at 650°C & oil quenched |
| UNS number | G41400 |
| US name | SAE H41400, SAE 4140, SAE 4142, SAE 4140, ASTM J 70, ASTM J 65, ASTM J 55, ASTM 4140, ASTM G41420, ASTM E7140, ASTM B7M, ASTM B16, ASTM 4142H, ASTM 4142, ASTM 4140H, ASTM 4140, ASTM 4137H, ASTM 41, ~SAE 4137H, ~ASTM B4D, ~ASTM 6 |
| EN name | ~42CrMoS4, ~42CrMo4 |
| EN number | ~1.7227, ~1.7223 |
| ISO name | ~ 42 CrMoS 4, ~ 42 CrMo 4, ~42CrMo4 |
| GB (Chinese) name | ~42CrMo |
| JIS (Japanese) name | SNB22-5, SNB22-4, SNB22-3, SNB22-2 |
AISI 4140 Oil Quenched & Tempered at 650°C Typical uses
| Heavy duty shafts, connecting rods, high tensile bolts, propeller shaft joints, track pins |
AISI 4140 Oil Quenched & Tempered at 650°C Composition detail
| C (carbon) | 0.38 | – | 0.43 | % |
| Cr (chromium) | 0.8 | – | 1.1 | % |
| Fe (iron) | 96.8 | – | 97.8 | % |
| Mn (manganese) | 0.75 | – | 1 | % |
| Mo (molybdenum) | 0.15 | – | 0.25 | % |
| P (phosphorus) | 0 | – | 0.035 | % |
| S (sulfur) | 0 | – | 0.04 | % |
| Si (silicon) | 0.15 | – | 0.35 | % |
AISI 4140 Oil Quenched & Tempered at 650°C Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 4140 Oil Quenched & Tempered at 650°C Mechanical properties
| Young’s modulus | 208 | – | 216 | GPa |
| Specific stiffness | 26.5 | – | 27.5 | MN.m/kg |
| Yield strength (elastic limit) | 595 | – | 715 | MPa |
| Tensile strength | 680 | – | 840 | MPa |
| Specific strength | 75.8 | – | 91.1 | kN.m/kg |
| Elongation | 17 | – | 27 | % strain |
| Compressive strength | 595 | – | 715 | MPa |
| Flexural modulus | 208 | – | 216 | GPa |
| Flexural strength (modulus of rupture) | 595 | – | 715 | MPa |
| Shear modulus | 80 | – | 85 | GPa |
| Bulk modulus | 161 | – | 176 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 39 | |||
| Hardness – Vickers | 210 | – | 260 | HV |
| Elastic stored energy (springs) | 841 | – | 1200 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 326 | – | 379 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 283 | – | 437 | MPa |
AISI 4140 Oil Quenched & Tempered at 650°C Impact & fracture properties
| Fracture toughness | 50 | – | 80 | MPa.m0.5 |
| Toughness (G) | 12.3 | – | 28.9 | kJ/m2 |
AISI 4140 Oil Quenched & Tempered at 650°C Thermal properties
| Melting point | 1430 | – | 1500 | °C |
| Maximum service temperature | 610 | – | 640 | °C |
| Minimum service temperature | -73 | – | -43 | °C |
| Thermal conductivity | 42 | – | 48 | W/m.°C |
| Specific heat capacity | 450 | – | 490 | J/kg.°C |
| Thermal expansion coefficient | 11.5 | – | 13.5 | µstrain/°C |
| Thermal shock resistance | 219 | – | 279 | °C |
| Thermal distortion resistance | 3.25 | – | 3.99 | MW/m |
| Latent heat of fusion | 265 | – | 280 | kJ/kg |
AISI 4140 Oil Quenched & Tempered at 650°C Electrical properties
| Electrical resistivity | 20 | – | 25 | µohm.cm |
| Electrical conductivity | 6.9 | – | 8.62 | %IACS |
| Galvanic potential | -0.5 | – | -0.42 | V |
AISI 4140 Oil Quenched & Tempered at 650°C Magnetic properties
| Magnetic type | Magnetic |
AISI 4140 Oil Quenched & Tempered at 650°C Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5140 | – | 5250 | m/s |
| Mechanical loss coefficient (tan delta) | 5.4e-4 | – | 6.7e-4 | |
AISI 4140 Oil Quenched & Tempered at 650°C Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Excellent |
| Metal hot forming | Excellent |
| Metal press forming | Excellent |
| Metal deep drawing | Limited use |
| Machining speed | 21.3 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Good |
| Carbon equivalency | 0.695 – 0.867 |
AISI 4140 Oil Quenched & Tempered at 650°C Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) | Acceptable |
| Flammability | Non-flammable |
AISI 4140 Oil Quenched & Tempered at 650°C Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments | Slightly susceptible |
AISI 4140 Oil Quenched & Tempered at 650°C Notes
| AISI 4140 Oil Quenched & Tempered at 650°C Other notes |
| Wear resistant – may be nitrided for extreme surface hardness. Tempering at high temperatures gives high tensile strength, good ductility and shock resistance. |
AISI 4140 Oil Quenched & Tempered at 650°C Standards with similar compositions
| Argentina: IRAM 4140 to IAS |
| Australia: 4140 to AS 1444, 4140H to AS 1444 |
| Finland: Co.42Cr1.1Mo0.20 to SFS 460 |
| France: 42CD4 to AFNOR NF A35-552, 42CD4 to AFNOR NF A35-553, 42CD4 to AFNOR NF A35-556, 42CD4 to AFNOR NF A35-557, 42CDTS to AFNOR NF A35-552, 42CDTS to AFNOR NF A35-553, 42CDTS to AFNOR NF A35-556, 42CDTS to AFNOR NF A35-557 |
| Germany: 1.7225 to DIN 1652, 42CrMo4 to DIN 1652, 42CrMo4 to DIN EN 10083 |
| Hungary: CMo4 to MSZ 61, CMo4E to MSZ 61, CMo4Z to MSZ 6251 |
| India: 40Cr4Mo2 to IS 13352, 42Cr4Mo2 to IS 1570/4, 43Cr4Mo2 to IS 14331 |
| International: 42CrMo4 to ISO 683-1, 42CrMo4 to ISO 683-18, 42CrMo4E to ISO 4954, 42CrMoS4 to ISO 683-1, 42CrMoS4 to ISO 683-18, Type 3a to ISO 683-4 |
| Italy: 40CrMo4 to UNI 5332, 41CrMo4 to UNI 8551, 42CrMo4 to UNI 6403, 42CrMo4 to UNI 7845, 42CrMo4 to UNI 7874, G40CrMo4 to UNI 3160 |
| Japan: SCM 4 to JIS G4105, SCM4H to JIS G4052, SNB22-1 to JIS G4108, SNB22-2 to JIS G4108, SNB22-3 to JIS G4108, SNB22-4 to JIS G4108, SNB22-5 to JIS G4108, SNB7 Class 2 to JIS G4107 |
| Mexico: 4140 to NMX-B-203-SCFI, 4140 to NMX-B-300, 4140H to NMX-B-268, 4140H to NMX-B-300, 4142 to NMX-B-300, 4142H to NMX-B-268, 4142H to NMX-B-300 |
| Norway: CrMoIV to NS |
| Pan America: 4140 to COPANT 334, 4140 to COPANT 514, 4142 to COPANT 514 |
| Romania: 42MoCr11 to STAS 791, 42MoCr11S to STAS 791, 42MoCr11X to STAS 791, 42MoCr11XS to STAS 791 |
| Serbia and Montenegro: C.4732, C.4782 |
| South Korea: SCM 440 H to KS D 3754 |
| Spain: 40CrMo4 to UNE 36012, F.1252 to UNE 36012 |
| Sweden: 2244 to SS 142244 |
| UK: 42CrMo4 to BS EN 10083-1, 42CrMo4 to BS EN 10132-3, 42CrMo4 to BS EN 10250-3, 42CrMo4 to BS EN 10269, 42CrMo4 to BS EN 10297-1, 5/2 to BS 3111/1, 708M40 to BS 970/3, 709M40 to BS 970/3 |
| USA: 4140 to ASTM A29/A29M, 4140 to ASTM A331-95, 4140 to ASTM A513, 4140 to ASTM A519, 4140 to ASTM A829/A829M, 4140 to DoD-F-24669/1, 4140 to FED QQ-S-626C, 4140 to SAE J404, 4140 to SAE J770, 4142 to ASTM A29/A29M, 4142 to ASTM A331-95, 4142 to ASTM A519, 4142 to ASTM A829/A829M, 4142 to SAE J404, 4145 to SAE J404, 7M to ASTM A194/A194M, B22 to ASTM A540/A540M, B7 to ASTM A193/A193M, B7M to ASTM A193/A193M, Class 3 to MIL-S-19434B, G41400 to ASTM A1031, G41400 to ASTM A506, G41400 to MIL-S-46059, G41420 to ASTM A1031, Grade 12 to ASTM A646-95, Grade 4 to ASTM A983/A983M, Grade 5 to ASTM A983/A983M, Grade 7 to ASTM A194/A194M, Grade J Class 110 to ASTM A372/A372M, Grade J Class 55 to ASTM A372/A372M, Grade J Class 65 to ASTM A372/A372M, Grade J Class 70 to ASTM A372/A372M, H41400 to SAE J775, L7 to ASTM A320/A320M, L70 to ASTM A320/A320M, L7M to ASTM A320/A320M, NV7 to SAE J775, UNS G41400, UNS G41420, UNS H41400, UNS H41420, UNS K14044, UNS K14047, UNS K14048, UNS K14245, UNS K14248 |
| Tradenames: 4140 FLAME DIE, A-1252, ASCOMETAL 42CD4, E.T.D. 150, E.T.D. 180, FAGERSTA C 345, KRUPP 42 CRMOS 4, LASALLE 4140, OVAKO 327, POMPEY 4142, POMPEY KD 39, RYCROME, SAARSTAHL 42 CRMO 4, STRAIN TEMPERED 4140, TKS 42CRMO4, VL-40 |