AISI 4140 Oil Quenched & Tempered at 315°C Material Data Sheet

AISI 4140 Oil Quenched & Tempered at 315°C Material Data Sheet

AISI 4140 Oil Quenched & Tempered at 315°C Overview

AISI 4140 tempered 315°C is AISI 4140 low alloy steel (UNS G41400, EN 42CrMo4) in the oil quenched & tempered at 315°C condition. This AISI 4140 tempered 315°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 4140 conditions in our AISI 4140 yield, tensile and hardness comparison. Looking for AISI 4140 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 4140 steel parts in-house and inspects them before shipment.

AISI 4140 Oil Quenched & Tempered at 315°C Designation

AISI 4140
ConditionTempered at 315°C & oil quenched
UNS numberG41400
US nameSAE H41400, SAE 4140, SAE 4142, SAE 4140, ASTM J 70, ASTM J 65, ASTM J 55, ASTM 4140, ASTM G41420, ASTM E7140, ASTM B7M, ASTM B16, ASTM 4142H, ASTM 4142, ASTM 4140H, ASTM 4140, ASTM 4137H, ASTM 41, ~SAE 4137H, ~ASTM B4D, ~ASTM 6
EN name~42CrMoS4, ~42CrMo4
EN number~1.7227, ~1.7223
ISO name~ 42 CrMoS 4, ~ 42 CrMo 4, ~42CrMo4
GB (Chinese) name~42CrMo
JIS (Japanese) nameSNB22-5, SNB22-4, SNB22-3, SNB22-2

AISI 4140 Oil Quenched & Tempered at 315°C Typical uses

Heavy duty shafts, connecting rods, high tensile bolts, propeller shaft joints, track pins

AISI 4140 Oil Quenched & Tempered at 315°C Composition detail

C (carbon)0.38–0.43%
Cr (chromium)0.8–1.1%
Fe (iron)96.8–97.8%
Mn (manganese)0.75–1%
Mo (molybdenum)0.15–0.25%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 4140 Oil Quenched & Tempered at 315°C Physical properties

Density7.8–7.9g/cm3

AISI 4140 Oil Quenched & Tempered at 315°C Mechanical properties

Young’s modulus208–216GPa
Specific stiffness26.5–27.5MN.m/kg
Yield strength (elastic limit)1290–1580MPa
Tensile strength1400–1710MPa
Specific strength164–201kN.m/kg
Elongation7–11% strain
Compressive strength1290–1580MPa
Flexural modulus208–216GPa
Flexural strength (modulus of rupture)1290–1580MPa
Shear modulus80–85GPa
Bulk modulus161–176GPa
Poisson’s ratio0.285–0.295 
Shape factor17
Hardness – Vickers400–490HV
Elastic stored energy (springs)3930–5840kJ/m3
Fatigue strength at 10^7 cycles540–622MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
473–710MPa

AISI 4140 Oil Quenched & Tempered at 315°C Impact & fracture properties

Fracture toughness29–54MPa.m0.5
Toughness (G)4.27–12.8kJ/m2

AISI 4140 Oil Quenched & Tempered at 315°C Thermal properties

Melting point1430–1500°C
Maximum service temperature275–305°C
Minimum service temperature-53–-28°C
Thermal conductivity42–48W/m.°C
Specific heat capacity450–490J/kg.°C
Thermal expansion coefficient11.5–13.5µstrain/°C
Thermal shock resistance474–614°C
Thermal distortion resistance3.25–3.99MW/m
Latent heat of fusion265–280kJ/kg

AISI 4140 Oil Quenched & Tempered at 315°C Electrical properties

Electrical resistivity20–25µohm.cm
Electrical conductivity6.9–8.62%IACS
Galvanic potential-0.5–-0.42V

AISI 4140 Oil Quenched & Tempered at 315°C Magnetic properties

Magnetic typeMagnetic

AISI 4140 Oil Quenched & Tempered at 315°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5140–5250m/s
Mechanical loss coefficient (tan delta)2.5e-4–3.2e-4 

AISI 4140 Oil Quenched & Tempered at 315°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed10.4 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.695 – 0.867

AISI 4140 Oil Quenched & Tempered at 315°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 4140 Oil Quenched & Tempered at 315°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Susceptible

AISI 4140 Oil Quenched & Tempered at 315°C Notes

AISI 4140 Oil Quenched & Tempered at 315°C Other notes
Wear resistant – may be nitrided for extreme surface hardness. Tempering at high temperatures gives high tensile strength, good ductility and shock resistance.

AISI 4140 Oil Quenched & Tempered at 315°C Standards with similar compositions

Argentina: IRAM 4140 to IAS
Australia: 4140 to AS 1444, 4140H to AS 1444
Finland: Co.42Cr1.1Mo0.20 to SFS 460
France: 42CD4 to AFNOR NF A35-552, 42CD4 to AFNOR NF A35-553, 42CD4 to AFNOR NF A35-556, 42CD4 to AFNOR NF A35-557, 42CDTS to AFNOR NF A35-552, 42CDTS to AFNOR NF A35-553, 42CDTS to AFNOR NF A35-556, 42CDTS to AFNOR NF A35-557
Germany: 1.7225 to DIN 1652, 42CrMo4 to DIN 1652, 42CrMo4 to DIN EN 10083
Hungary: CMo4 to MSZ 61, CMo4E to MSZ 61, CMo4Z to MSZ 6251
India: 40Cr4Mo2 to IS 13352, 42Cr4Mo2 to IS 1570/4, 43Cr4Mo2 to IS 14331
International: 42CrMo4 to ISO 683-1, 42CrMo4 to ISO 683-18, 42CrMo4E to ISO 4954, 42CrMoS4 to ISO 683-1, 42CrMoS4 to ISO 683-18, Type 3a to ISO 683-4
Italy: 40CrMo4 to UNI 5332, 41CrMo4 to UNI 8551, 42CrMo4 to UNI 6403, 42CrMo4 to UNI 7845, 42CrMo4 to UNI 7874, G40CrMo4 to UNI 3160
Japan: SCM 4 to JIS G4105, SCM4H to JIS G4052, SNB22-1 to JIS G4108, SNB22-2 to JIS G4108, SNB22-3 to JIS G4108, SNB22-4 to JIS G4108, SNB22-5 to JIS G4108, SNB7 Class 2 to JIS G4107
Mexico: 4140 to NMX-B-203-SCFI, 4140 to NMX-B-300, 4140H to NMX-B-268, 4140H to NMX-B-300, 4142 to NMX-B-300, 4142H to NMX-B-268, 4142H to NMX-B-300
Norway: CrMoIV to NS
Pan America: 4140 to COPANT 334, 4140 to COPANT 514, 4142 to COPANT 514
Romania: 42MoCr11 to STAS 791, 42MoCr11S to STAS 791, 42MoCr11X to STAS 791, 42MoCr11XS to STAS 791
Serbia and Montenegro: C.4732, C.4782
South Korea: SCM 440 H to KS D 3754
Spain: 40CrMo4 to UNE 36012, F.1252 to UNE 36012
Sweden: 2244 to SS 142244
UK: 42CrMo4 to BS EN 10083-1, 42CrMo4 to BS EN 10132-3, 42CrMo4 to BS EN 10250-3, 42CrMo4 to BS EN 10269, 42CrMo4 to BS EN 10297-1, 5/2 to BS 3111/1, 708M40 to BS 970/3, 709M40 to BS 970/3
USA: 4140 to ASTM A29/A29M, 4140 to ASTM A331-95, 4140 to ASTM A513, 4140 to ASTM A519, 4140 to ASTM A829/A829M, 4140 to DoD-F-24669/1, 4140 to FED QQ-S-626C, 4140 to SAE J404, 4140 to SAE J770, 4142 to ASTM A29/A29M, 4142 to ASTM A331-95, 4142 to ASTM A519, 4142 to ASTM A829/A829M, 4142 to SAE J404, 4145 to SAE J404, 7M to ASTM A194/A194M, B22 to ASTM A540/A540M, B7 to ASTM A193/A193M, B7M to ASTM A193/A193M, Class 3 to MIL-S-19434B, G41400 to ASTM A1031, G41400 to ASTM A506, G41400 to MIL-S-46059, G41420 to ASTM A1031, Grade 12 to ASTM A646-95, Grade 4 to ASTM A983/A983M, Grade 5 to ASTM A983/A983M, Grade 7 to ASTM A194/A194M, Grade J Class 110 to ASTM A372/A372M, Grade J Class 55 to ASTM A372/A372M, Grade J Class 65 to ASTM A372/A372M, Grade J Class 70 to ASTM A372/A372M, H41400 to SAE J775, L7 to ASTM A320/A320M, L70 to ASTM A320/A320M, L7M to ASTM A320/A320M, NV7 to SAE J775, UNS G41400, UNS G41420, UNS H41400, UNS H41420, UNS K14044, UNS K14047, UNS K14048, UNS K14245, UNS K14248
Tradenames: 4140 FLAME DIE, A-1252, ASCOMETAL 42CD4, E.T.D. 150, E.T.D. 180, FAGERSTA C 345, KRUPP 42 CRMOS 4, LASALLE 4140, OVAKO 327, POMPEY 4142, POMPEY KD 39, RYCROME, SAARSTAHL 42 CRMO 4, STRAIN TEMPERED 4140, TKS 42CRMO4, VL-40