AISI 9310 Annealed vs Normalized: Yield, Tensile & Hardness Compared

How do the AISI 9310 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 9310 (UNS G93100, EN 14NiCrMo13-4) side by side for 2 conditions: Annealed, Normalized. All values are taken from the individual AISI 9310 material data sheets linked below.

AISI 9310 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Annealed400–480735–905220–27013–21
Normalized510–630815–1000248–30315–23

AISI 9310 Differences Compared with Annealed

The table below shows how much each condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Normalized+30%+11%+12%+12%

AISI 9310 Strength and Hardness Charts

AISI 9310 Yield strength (MPa)Annealed400–480Normalized510–630
AISI 9310 Tensile strength (MPa)Annealed735–905Normalized815–1000
AISI 9310 Hardness (HV)Annealed220–270Normalized248–303

AISI 9310 Heat Treatment Key Points

The highest tensile strength is reached in the normalized condition (815–1000 MPa). The softest condition is annealed (220–270 HV), which is usually preferred for machining and forming.

AISI 9310 Material Data Sheets

AISI 9310 Annealed | AISI 9310 Normalized | All AISI 9310 conditions