AISI 9310 Annealed Material Data Sheet

AISI 9310 Annealed Material Data Sheet

AISI 9310 Annealed Overview

AISI 9310 annealed is AISI 9310 low alloy steel (UNS G93100, EN 14NiCrMo13-4) in the annealed condition. This AISI 9310 annealed material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 9310 conditions in our AISI 9310 yield, tensile and hardness comparison. Looking for AISI 9310 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 9310 steel parts in-house and inspects them before shipment.

AISI 9310 Annealed Designation

AISI 9310
ConditionAnnealed
UNS numberG93100, G93106
US nameASTM A29 E9310, ASTM A646 Grade 2, AMS 6260, AMS 6267, AMS 6263
EN nameBS S 157, 14NiCrMo13-4, 832M13, EN36C, 16NCD13
EN number1.6657, 1.6658

AISI 9310 Annealed Typical uses

Heavy duty aircraft, vehicle transmission gears, track rod pins, roller bearing rings, small arms parts

AISI 9310 Annealed Composition detail

C (carbon)0.08–0.13%
Cr (chromium)1–1.4%
Fe (iron)93.8–95.2%
Mn (manganese)0.45–0.65%
Mo (molybdenum)0.08–0.15%
Ni (nickel)3–3.5%
P (phosphorus)0–0.025%
S (sulfur)0–0.025%
Si (silicon)0.15–0.35%

AISI 9310 Annealed Physical properties

Density7.8–7.9g/cm3

AISI 9310 Annealed Mechanical properties

Young’s modulus206–216GPa
Specific stiffness26.2–27.5MN.m/kg
Yield strength (elastic limit)400–480MPa
Tensile strength735–905MPa
Specific strength50.9–61.2kN.m/kg
Elongation13–21% strain
Compressive strength400–480MPa
Flexural modulus206–216GPa
Flexural strength (modulus of rupture)400–480MPa
Shear modulus79–85GPa
Bulk modulus159–176GPa
Poisson’s ratio0.285–0.295 
Shape factor52
Hardness – Vickers220–270HV
Elastic stored energy (springs)382–543kJ/m3
Fatigue strength at 10^7 cycles345–400MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
300–460MPa

AISI 9310 Annealed Impact & fracture properties

Fracture toughness90–138MPa.m0.5
Toughness (G)39.9–87kJ/m2

AISI 9310 Annealed Thermal properties

Melting point1490–1530°C
Maximum service temperature644–665°C
Minimum service temperature-68–-43°C
Thermal conductivity46–51W/m.°C
Specific heat capacity425–475J/kg.°C
Thermal expansion coefficient11–13µstrain/°C
Thermal shock resistance154–197°C
Thermal distortion resistance3.68–4.46MW/m
Latent heat of fusion265–280kJ/kg

AISI 9310 Annealed Electrical properties

Electrical resistivity15–35µohm.cm
Electrical conductivity4.93–11.5%IACS
Galvanic potential-0.49–-0.41V

AISI 9310 Annealed Magnetic properties

Magnetic typeMagnetic

AISI 9310 Annealed Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5120–5250m/s
Mechanical loss coefficient (tan delta)6.3e-4–7.8e-4 

AISI 9310 Annealed Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed18.6 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Excellent
Carbon equivalency0.189 – 0.278

AISI 9310 Annealed Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 9310 Annealed Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 9310 Annealed Notes

AISI 9310 Annealed Other notes
Gives good impact properties in the thicker sections and is tolerant of limitations in heat treatment technique.

AISI 9310 Annealed Standards with similar compositions

China: G10CrNi3Mo to GB 3203
Italy: 10NiCrMo13 to UNI 6935
Mexico: 9310H to NMX-B-268, 9310H to NMX-B-300, E9310 to NMX-B-300
UK: 14NiCrMo13-4 to BS EN 10084, 655H13 to BS 970/1, 655M13 to BS 970/3, 832H13 to BS 970/1, 832M13 to BS 970/1
USA: 9310, 9310H, 9310H to ASTM A304, 9310H to ASTM A331-95, 9310H to ASTM A534, 9310RH to ASTM A914/A914M-92, 9310RH to SAE J1868, 9315, E9310 to ASTM A1031, E9310 to ASTM A29/A29M, E9310 to ASTM A519, E9310H to SAE J1268, G93100 to ASTM A837/A837M, Grade 2 to ASTM A646-95, UNS G93106, UNS H93100, UNS H93106, UNS K44414
Tradenames: VA-15, VASCO 9310