AISI 9310 normalized is AISI 9310 low alloy steel (UNS G93100, EN 14NiCrMo13-4) in the normalized condition. This AISI 9310 normalized material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 9310 conditions in our AISI 9310 yield, tensile and hardness comparison. Looking for AISI 9310 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 9310 steel parts in-house and inspects them before shipment.
Heavy duty aircraft, vehicle transmission gears, track rod pins, roller bearing rings, small arms parts
AISI 9310 Normalized Composition detail
C (carbon)
0.08
–
0.13
%
Cr (chromium)
1
–
1.4
%
Fe (iron)
93.8
–
95.2
%
Mn (manganese)
0.45
–
0.65
%
Mo (molybdenum)
0.08
–
0.15
%
Ni (nickel)
3
–
3.5
%
P (phosphorus)
0
–
0.025
%
S (sulfur)
0
–
0.025
%
Si (silicon)
0.15
–
0.35
%
AISI 9310 Normalized Physical properties
Density
7.8
–
7.9
g/cm3
AISI 9310 Normalized Mechanical properties
Young’s modulus
206
–
216
GPa
Specific stiffness
26.2
–
27.5
MN.m/kg
Yield strength (elastic limit)
510
–
630
MPa
Tensile strength
815
–
1000
MPa
Specific strength
65
–
80.3
kN.m/kg
Elongation
15
–
23
% strain
Compressive strength
510
–
630
MPa
Flexural modulus
206
–
216
GPa
Flexural strength (modulus of rupture)
510
–
630
MPa
Shear modulus
79
–
85
GPa
Bulk modulus
159
–
176
GPa
Poisson’s ratio
0.285
–
0.295
Shape factor
43
Hardness – Vickers
248
–
303
HV
Elastic stored energy (springs)
622
–
932
kJ/m3
Fatigue strength at 10^7 cycles
370
–
429
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
323
–
492
MPa
AISI 9310 Normalized Impact & fracture properties
Fracture toughness
71
–
114
MPa.m0.5
Toughness (G)
25
–
58.9
kJ/m2
AISI 9310 Normalized Thermal properties
Melting point
1490
–
1530
°C
Maximum service temperature
644
–
665
°C
Minimum service temperature
-68
–
-43
°C
Thermal conductivity
46
–
51
W/m.°C
Specific heat capacity
425
–
475
J/kg.°C
Thermal expansion coefficient
11
–
13
µstrain/°C
Thermal shock resistance
197
–
257
°C
Thermal distortion resistance
3.68
–
4.46
MW/m
Latent heat of fusion
265
–
280
kJ/kg
AISI 9310 Normalized Electrical properties
Electrical resistivity
15
–
35
µohm.cm
Electrical conductivity
4.93
–
11.5
%IACS
Temperature dependence of resistivity
10
–
11
/°C
Galvanic potential
-0.49
–
-0.41
V
AISI 9310 Normalized Magnetic properties
Magnetic type
Magnetic
AISI 9310 Normalized Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5120
–
5250
m/s
Mechanical loss coefficient (tan delta)
5.2e-4
–
6.6e-4
AISI 9310 Normalized Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
16.5 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Excellent
Carbon equivalency
0.189 – 0.278
AISI 9310 Normalized Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
AISI 9310 Normalized Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible
AISI 9310 Normalized Notes
AISI 9310 Normalized Other notes
Gives good impact properties in the thicker sections and is tolerant of limitations in heat treatment technique.
AISI 9310 Normalized Standards with similar compositions
China: G10CrNi3Mo to GB 3203
Italy: 10NiCrMo13 to UNI 6935
Mexico: 9310H to NMX-B-268, 9310H to NMX-B-300, E9310 to NMX-B-300
UK: 14NiCrMo13-4 to BS EN 10084, 655H13 to BS 970/1, 655M13 to BS 970/3, 832H13 to BS 970/1, 832M13 to BS 970/1
USA: 9310, 9310H, 9310H to ASTM A304, 9310H to ASTM A331-95, 9310H to ASTM A534, 9310RH to ASTM A914/A914M-92, 9310RH to SAE J1868, 9315, E9310 to ASTM A1031, E9310 to ASTM A29/A29M, E9310 to ASTM A519, E9310H to SAE J1268, G93100 to ASTM A837/A837M, Grade 2 to ASTM A646-95, UNS G93106, UNS H93100, UNS H93106, UNS K44414