How do the AISI 8740 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 8740 (UNS G87400) side by side for 8 conditions: Annealed, Normalized, Quenched & Tempered, Oil Quenched & Tempered at 205°C, Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 8740 material data sheets linked below.
AISI 8740 Yield, Tensile and Hardness by Condition
| Condition | Yield strength (MPa) | Tensile strength (MPa) | Hardness (HV) | Elongation (%) |
|---|---|---|---|---|
| Annealed | 370–460 | 625–765 | 185–230 | 18–26 |
| Normalized | 540–675 | 830–1030 | 248–303 | 12–20 |
| Quenched & Tempered | 690–763 | 862–953 | 370–460 | 17–19.8 |
| Oil Quenched & Tempered at 205°C | 1490–1820 | 1800–2200 | 518–638 | 8–12 |
| Oil Quenched & Tempered at 315°C | 1400–1710 | 1540–1900 | 445–545 | 9–13 |
| Oil Quenched & Tempered at 425°C | 1220–1500 | 1290–1580 | 370–460 | 10–16 |
| Oil Quenched & Tempered at 540°C | 1020–1260 | 1090–1330 | 325–405 | 12–18 |
| Oil Quenched & Tempered at 650°C | 810–995 | 885–1090 | 275–335 | 16–24 |
AISI 8740 Differences Compared with Annealed
The table below shows how much each condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength or hardness.
| Condition | Yield strength | Tensile strength | Hardness | Elongation |
|---|---|---|---|---|
| Normalized | +46% | +34% | +33% | -27% |
| Quenched & Tempered | +75% | +31% | +100% | -16% |
| Oil Quenched & Tempered at 205°C | +299% | +188% | +179% | -55% |
| Oil Quenched & Tempered at 315°C | +275% | +147% | +139% | -50% |
| Oil Quenched & Tempered at 425°C | +228% | +106% | +100% | -41% |
| Oil Quenched & Tempered at 540°C | +175% | +74% | +76% | -32% |
| Oil Quenched & Tempered at 650°C | +117% | +42% | +47% | -9% |
AISI 8740 Strength and Hardness Charts
AISI 8740 Heat Treatment Key Points
The highest tensile strength is reached in the oil quenched & tempered at 205°C condition (1800–2200 MPa). The softest condition is annealed (185–230 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 205°C to 650°C lowers hardness from 518–638 HV to 275–335 HV, trading strength for toughness and ductility.
AISI 8740 Material Data Sheets
AISI 8740 Annealed | AISI 8740 Normalized | AISI 8740 Quenched & Tempered | AISI 8740 Oil Quenched & Tempered at 205°C | AISI 8740 Oil Quenched & Tempered at 315°C | AISI 8740 Oil Quenched & Tempered at 425°C | AISI 8740 Oil Quenched & Tempered at 540°C | AISI 8740 Oil Quenched & Tempered at 650°C | All AISI 8740 conditions
Looking for AISI 8740 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 8740 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.