AISI 8740 normalized is AISI 8740 low alloy steel (UNS G87400) in the normalized condition. This AISI 8740 normalized material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 8740 conditions in our AISI 8740 yield, tensile and hardness comparison. Looking for AISI 8740 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 8740 steel parts in-house and inspects them before shipment.
General construction, general mechanical engineering, automotive, tools, axles, gears, springs.
AISI 8740 Normalized Composition detail
C (carbon)
0.38
–
0.43
%
Cr (chromium)
0.4
–
0.6
%
Fe (iron)
96.5
–
97.7
%
Mn (manganese)
0.75
–
1
%
Mo (molybdenum)
0.2
–
0.3
%
Ni (nickel)
0.4
–
0.7
%
P (phosphorus)
0
–
0.035
%
S (sulfur)
0
–
0.04
%
Si (silicon)
0.15
–
0.35
%
AISI 8740 Normalized Physical properties
Density
7.8
–
7.9
g/cm3
AISI 8740 Normalized Mechanical properties
Young’s modulus
201
–
212
GPa
Specific stiffness
25.6
–
27
MN.m/kg
Yield strength (elastic limit)
540
–
675
MPa
Tensile strength
830
–
1030
MPa
Specific strength
68.8
–
86
kN.m/kg
Elongation
12
–
20
% strain
Compressive strength
540
–
675
MPa
Flexural modulus
201
–
212
GPa
Flexural strength (modulus of rupture)
540
–
675
MPa
Shear modulus
77
–
83
GPa
Bulk modulus
155
–
173
GPa
Poisson’s ratio
0.285
–
0.295
Shape factor
40
Hardness – Vickers
248
–
303
HV
Elastic stored energy (springs)
713
–
1090
kJ/m3
Fatigue strength at 10^7 cycles
375
–
436
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
326
–
502
MPa
AISI 8740 Normalized Impact & fracture properties
Fracture toughness
66
–
109
MPa.m0.5
Toughness (G)
22.2
–
54.7
kJ/m2
AISI 8740 Normalized Thermal properties
Melting point
1430
–
1510
°C
Maximum service temperature
613
–
653
°C
Minimum service temperature
-68
–
-43
°C
Thermal conductivity
35
–
55
W/m.°C
Specific heat capacity
420
–
520
J/kg.°C
Thermal expansion coefficient
11
–
13
µstrain/°C
Thermal shock resistance
213
–
281
°C
Thermal distortion resistance
2.89
–
4.65
MW/m
Latent heat of fusion
265
–
280
kJ/kg
AISI 8740 Normalized Electrical properties
Electrical resistivity
23
–
35
µohm.cm
Electrical conductivity
4.93
–
7.5
%IACS
Galvanic potential
-0.51
–
-0.43
V
AISI 8740 Normalized Magnetic properties
Magnetic type
Magnetic
AISI 8740 Normalized Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5060
–
5200
m/s
Mechanical loss coefficient (tan delta)
5e-4
–
6.3e-4
AISI 8740 Normalized Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
17.4 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency
0.652 – 0.823
AISI 8740 Normalized Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
AISI 8740 Normalized Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible
AISI 8740 Normalized Standards with similar compositions
Australia: 8740 to AS 1444, 8740H to AS 1444
Belgium: 40NiCrMo2 to NBN 253-02
France: 40NCD2 to AFNOR, 40NCD2TS to AFNOR, 40NCD3TS to AFNOR
Germany: 40NiCrMo2-2 to DIN
Hungary: NCMo3 to MSZ 61, NCMo3E to MSZ 61, NCMo3Z to MSZ 6251
International: 1 to ISO 683-8, 10 to ISO 683-12, 1A to ISO 683-8, 1b to ISO 683-8, 41CrNiMo2 to ISO 683-1, 41CrNiMo2E to ISO 4954, 41CrNiMoS2 to ISO 683-1
Italy: 40NiCrMo2 to UNI 7874, 40NiCrMo2KB to UNI 7356
Japan: SNCM 240 to JIS G4053, SNCM240 to JIS G4103, SNCM240RCH to JIS G3509-1, SNCM6 to JIS G4103
Mexico: 8740 to NMX-B-300, 8740H to NMX-B-268, 8740H to NMX-B-300
Pan America: 8740 to COPANT 334
South Korea: SNCM 240 to KS D 3709
Spain: 40NiCrMo2 to UNE 36012, 40NiCrMo2DF to UNE 36034, F.1204 to UNE 36012, F.1205 to UNE 36034
UK: 7 to BS 3111/1
USA: 8740, 8740 to ASTM A29/A29M, 8740 to ASTM A322-91, 8740 to ASTM A331-95, 8740 to ASTM A519, 8740 to ASTM A752/A752M, 8740H, 8740H to ASTM A304, 8740H to ASTM A331-95, 8740H to SAE J1268, 8742, 8742 to ASTM A519, 8742 to ASTM A829/A829M, 8742 to SAE J404, G87400 to ASTM A1031, L73 to ASTM A320/A320M, L7C to ASTM A320/A320M, UNS G87400, UNS G87420, UNS H87400