AISI 8740 Quenched & Tempered Material Data Sheet

AISI 8740 Quenched & Tempered Material Data Sheet

AISI 8740 Quenched & Tempered Overview

AISI 8740 quenched tempered is AISI 8740 low alloy steel (UNS G87400) in the quenched & tempered condition. This AISI 8740 quenched tempered material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 8740 conditions in our AISI 8740 yield, tensile and hardness comparison. Looking for AISI 8740 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 8740 steel parts in-house and inspects them before shipment.

AISI 8740 Quenched & Tempered Designation

AISI 8740
ConditionQuenched & tempered
UNS numberG87400
US nameSAE 8740, ASTM G87400, ASTM 8740H, ASTM 8740, ASTM 8640H, ASTM 8640, ~SAE 8640
ISO name41CrNiMoS2, 1b, 1A, ~41CrNiMo2E, ~41CrNiMo2
JIS (Japanese) nameSNCM240

AISI 8740 Quenched & Tempered Typical uses

General construction, general mechanical engineering, automotive, pressure vessels, pipework

AISI 8740 Quenched & Tempered Composition detail

C (carbon)0.38–0.43%
Cr (chromium)0.4–0.6%
Fe (iron)96.5–97.7%
Mn (manganese)0.75–1%
Mo (molybdenum)0.2–0.3%
Ni (nickel)0.4–0.7%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 8740 Quenched & Tempered Physical properties

Density7.79–7.87g/cm3

AISI 8740 Quenched & Tempered Mechanical properties

Young’s modulus200–210GPa
Specific stiffness25.5–26.9MN.m/kg
Yield strength (elastic limit)690–763MPa
Tensile strength862–953MPa
Specific strength88.1–97.4kN.m/kg
Elongation17–19.8% strain
Compressive strength745–823MPa
Flexural modulus200–210GPa
Flexural strength (modulus of rupture)690–763MPa
Shear modulus76–79.9GPa
Bulk modulus185–195GPa
Poisson’s ratio0.32–0.333 
Shape factor34
Hardness – Vickers370–460HV
Elastic stored energy (springs)1160–1420kJ/m3
Fatigue strength at 10^7 cycles510–590MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
486–619MPa

AISI 8740 Quenched & Tempered Impact & fracture properties

Fracture toughness30–54MPa.m0.5
Toughness (G)4.69–13.3kJ/m2

AISI 8740 Quenched & Tempered Thermal properties

Melting point1430–1510°C
Maximum service temperature495–552°C
Minimum service temperature-58–-28°C
Thermal conductivity55–59.6W/m.°C
Specific heat capacity461–480J/kg.°C
Thermal expansion coefficient12.4–13.1µstrain/°C
Thermal shock resistance261–295°C
Thermal distortion resistance4.29–4.71MW/m
Latent heat of fusion265–280kJ/kg

AISI 8740 Quenched & Tempered Electrical properties

Electrical resistivity23–35µohm.cm
Electrical conductivity4.93–7.5%IACS
Galvanic potential-0.51–-0.43V

AISI 8740 Quenched & Tempered Magnetic properties

Magnetic typeMagnetic

AISI 8740 Quenched & Tempered Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5050–5180m/s
Mechanical loss coefficient (tan delta)2e-4–5e-4 

AISI 8740 Quenched & Tempered Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed13.4 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.652 – 0.823

AISI 8740 Quenched & Tempered Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 8740 Quenched & Tempered Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 8740 Quenched & Tempered Notes

AISI 8740 Quenched & Tempered Warning
Some rare heat treatments of certain alloys may produce values for mechanical properties outside the given ranges, e.g. AISI 9255. tempered at 205C

AISI 8740 Quenched & Tempered Standards with similar compositions

Australia: 8740 to AS 1444, 8740H to AS 1444
Belgium: 40NiCrMo2 to NBN 253-02
France: 40NCD2 to AFNOR, 40NCD2TS to AFNOR, 40NCD3TS to AFNOR
Germany: 40NiCrMo2-2 to DIN
Hungary: NCMo3 to MSZ 61, NCMo3E to MSZ 61, NCMo3Z to MSZ 6251
International: 1 to ISO 683-8, 10 to ISO 683-12, 1A to ISO 683-8, 1b to ISO 683-8, 41CrNiMo2 to ISO 683-1, 41CrNiMo2E to ISO 4954, 41CrNiMoS2 to ISO 683-1
Italy: 40NiCrMo2 to UNI 7874, 40NiCrMo2KB to UNI 7356
Japan: SNCM 240 to JIS G4053, SNCM240 to JIS G4103, SNCM240RCH to JIS G3509-1, SNCM6 to JIS G4103
Mexico: 8740 to NMX-B-300, 8740H to NMX-B-268, 8740H to NMX-B-300
Pan America: 8740 to COPANT 334
South Korea: SNCM 240 to KS D 3709
Spain: 40NiCrMo2 to UNE 36012, 40NiCrMo2DF to UNE 36034, F.1204 to UNE 36012, F.1205 to UNE 36034
UK: 7 to BS 3111/1
USA: 8740, 8740 to ASTM A29/A29M, 8740 to ASTM A322-91, 8740 to ASTM A331-95, 8740 to ASTM A519, 8740 to ASTM A752/A752M, 8740H, 8740H to ASTM A304, 8740H to ASTM A331-95, 8740H to SAE J1268, 8742, 8742 to ASTM A519, 8742 to ASTM A829/A829M, 8742 to SAE J404, G87400 to ASTM A1031, L73 to ASTM A320/A320M, L7C to ASTM A320/A320M, UNS G87400, UNS G87420, UNS H87400
Tradenames: A-1204, KRUPP 40 NICRMO 2 2