AISI 8650 Annealed vs Normalized vs Quenched & Tempered (205–650°C): Yield, Tensile & Hardness Compared

How do the AISI 8650 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 8650 (UNS G86500) side by side for 7 conditions: Annealed, Normalized, Oil Quenched & Tempered at 205°C, Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 8650 material data sheets linked below.

AISI 8650 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Annealed340–405640–790193–24318–27
Normalized615–760915–1130275–33511–17
Oil Quenched & Tempered at 205°C1500–18501740–2140470–5808–12
Oil Quenched & Tempered at 315°C1400–17101550–1900440–5408–12
Oil Quenched & Tempered at 425°C1190–14601300–1600375–4659–15
Oil Quenched & Tempered at 540°C945–11601060–1290305–37512–18
Oil Quenched & Tempered at 650°C745–910865–1070250–31016–24

AISI 8650 Differences Compared with Annealed

The table below shows how much each condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Normalized+85%+43%+40%-38%
Oil Quenched & Tempered at 205°C+350%+171%+141%-56%
Oil Quenched & Tempered at 315°C+317%+141%+125%-56%
Oil Quenched & Tempered at 425°C+256%+103%+93%-47%
Oil Quenched & Tempered at 540°C+183%+64%+56%-33%
Oil Quenched & Tempered at 650°C+122%+35%+28%-11%

AISI 8650 Strength and Hardness Charts

AISI 8650 Yield strength (MPa)Annealed340–405Normalized615–760Q&T 205°C1500–1850Q&T 315°C1400–1710Q&T 425°C1190–1460Q&T 540°C945–1160Q&T 650°C745–910
AISI 8650 Tensile strength (MPa)Annealed640–790Normalized915–1130Q&T 205°C1740–2140Q&T 315°C1550–1900Q&T 425°C1300–1600Q&T 540°C1060–1290Q&T 650°C865–1070
AISI 8650 Hardness (HV)Annealed193–243Normalized275–335Q&T 205°C470–580Q&T 315°C440–540Q&T 425°C375–465Q&T 540°C305–375Q&T 650°C250–310

AISI 8650 Heat Treatment Key Points

The highest tensile strength is reached in the oil quenched & tempered at 205°C condition (1740–2140 MPa). The softest condition is annealed (193–243 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 205°C to 650°C lowers hardness from 470–580 HV to 250–310 HV, trading strength for toughness and ductility.

AISI 8650 Material Data Sheets

AISI 8650 Annealed | AISI 8650 Normalized | AISI 8650 Oil Quenched & Tempered at 205°C | AISI 8650 Oil Quenched & Tempered at 315°C | AISI 8650 Oil Quenched & Tempered at 425°C | AISI 8650 Oil Quenched & Tempered at 540°C | AISI 8650 Oil Quenched & Tempered at 650°C | All AISI 8650 conditions