AISI 8650 annealed is AISI 8650 low alloy steel (UNS G86500) in the annealed condition. This AISI 8650 annealed material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 8650 conditions in our AISI 8650 yield, tensile and hardness comparison. Looking for AISI 8650 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 8650 steel parts in-house and inspects them before shipment.
General construction, general mechanical engineering, automotive, tools, axles, gears, springs.
AISI 8650 Annealed Composition detail
C (carbon)
0.48
–
0.53
%
Cr (chromium)
0.4
–
0.6
%
Fe (iron)
96.5
–
97.7
%
Mn (manganese)
0.75
–
1
%
Mo (molybdenum)
0.15
–
0.25
%
Ni (nickel)
0.4
–
0.7
%
P (phosphorus)
0
–
0.035
%
S (sulfur)
0
–
0.04
%
Si (silicon)
0.15
–
0.35
%
AISI 8650 Annealed Physical properties
Density
7.8
–
7.9
g/cm3
AISI 8650 Annealed Mechanical properties
Young’s modulus
206
–
216
GPa
Specific stiffness
26.2
–
27.5
MN.m/kg
Yield strength (elastic limit)
340
–
405
MPa
Tensile strength
640
–
790
MPa
Specific strength
43.3
–
51.6
kN.m/kg
Elongation
18
–
27
% strain
Compressive strength
340
–
405
MPa
Flexural modulus
206
–
216
GPa
Flexural strength (modulus of rupture)
340
–
405
MPa
Shear modulus
79
–
85
GPa
Bulk modulus
159
–
176
GPa
Poisson’s ratio
0.285
–
0.295
Shape factor
57
Hardness – Vickers
193
–
243
HV
Elastic stored energy (springs)
276
–
387
kJ/m3
Fatigue strength at 10^7 cycles
313
–
363
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
272
–
418
MPa
AISI 8650 Annealed Impact & fracture properties
Fracture toughness
95
–
145
MPa.m0.5
Toughness (G)
44.4
–
96.1
kJ/m2
AISI 8650 Annealed Thermal properties
Melting point
1410
–
1500
°C
Maximum service temperature
601
–
648
°C
Minimum service temperature
-73
–
-43
°C
Thermal conductivity
35
–
45
W/m.°C
Specific heat capacity
460
–
500
J/kg.°C
Thermal expansion coefficient
11
–
12.5
µstrain/°C
Thermal shock resistance
135
–
167
°C
Thermal distortion resistance
2.94
–
3.89
MW/m
Latent heat of fusion
265
–
280
kJ/kg
AISI 8650 Annealed Electrical properties
Electrical resistivity
23
–
35
µohm.cm
Electrical conductivity
4.93
–
7.5
%IACS
Galvanic potential
-0.5
–
-0.42
V
AISI 8650 Annealed Magnetic properties
Magnetic type
Magnetic
AISI 8650 Annealed Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5120
–
5250
m/s
Mechanical loss coefficient (tan delta)
7.4e-4
–
9.1e-4
AISI 8650 Annealed Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
22.6 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency
0.742 – 0.913
AISI 8650 Annealed Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
AISI 8650 Annealed Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible
AISI 8650 Annealed Standards with similar compositions
Mexico: 8650 to NMX-B-203-SCFI, 8650 to NMX-B-300, 8650H to NMX-B-268, 8650H to NMX-B-300, 8655 to NMX-B-203-SCFI, 8655 to NMX-B-300, 8655H to NMX-B-268, 8655H to NMX-B-300
Pan America: 8650 to COPANT 334, 8650 to COPANT 514
USA: 8650, 8650 to ASTM A29/A29M, 8650 to ASTM A322-91, 8650 to ASTM A331-95, 8650 to ASTM A519, 8650 to SAE J770, 8650H, 8650H to ASTM A304, 8650H to ASTM A331-95, 8650H to SAE J1268, 8653, 8655, 8655 to ASTM A29/A29M, 8655 to ASTM A322-91, 8655 to ASTM A331-95, 8655 to ASTM A519, 8655 to ASTM A752/A752M, 8655 to ASTM A829/A829M, 8655 to SAE J404, 8655 to SAE J770, 8655H, 8655H to ASTM A304, 8655H to ASTM A331-95, 8655H to SAE J1268, 8750, G86500 to ASTM A1031, G86550 to ASTM A1031, UNS G86500, UNS G86550, UNS H86500, UNS H86550, UNS K13550