AISI 8630 Annealed vs Normalized vs Quenched & Tempered (205–650°C): Yield, Tensile & Hardness Compared

How do the AISI 8630 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 8630 (UNS G86300, EN 30NiCrMo2-2) side by side for 8 conditions: Annealed, Normalized, Air Melted, Quenched & Tempered, Oil Quenched & Tempered at 205°C, Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 8630 material data sheets linked below.

AISI 8630 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Annealed335–410500–625145–18023–35
Normalized483–534621–686173–2136–15
Air Melted, Quenched & Tempered690–763862–953220–27017–19.8
Oil Quenched & Tempered at 205°C1350–16601480–1810415–5157–11
Oil Quenched & Tempered at 315°C1250–15401330–1640385–4758–12
Oil Quenched & Tempered at 425°C1050–13001150–1410340–41510–16
Oil Quenched & Tempered at 540°C805–990925–1140280–34513–21
Oil Quenched & Tempered at 650°C620–760690–855220–27018–28

AISI 8630 Differences Compared with Annealed

The table below shows how much each condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Normalized+37%+16%+19%-64%
Air Melted, Quenched & Tempered+95%+61%+51%-37%
Oil Quenched & Tempered at 205°C+304%+192%+186%-69%
Oil Quenched & Tempered at 315°C+274%+164%+165%-66%
Oil Quenched & Tempered at 425°C+215%+128%+132%-55%
Oil Quenched & Tempered at 540°C+141%+84%+92%-41%
Oil Quenched & Tempered at 650°C+85%+37%+51%-21%

AISI 8630 Strength and Hardness Charts

AISI 8630 Yield strength (MPa)Annealed335–410Normalized483–534Air Melted, Q&T690–763Q&T 205°C1350–1660Q&T 315°C1250–1540Q&T 425°C1050–1300Q&T 540°C805–990Q&T 650°C620–760
AISI 8630 Tensile strength (MPa)Annealed500–625Normalized621–686Air Melted, Q&T862–953Q&T 205°C1480–1810Q&T 315°C1330–1640Q&T 425°C1150–1410Q&T 540°C925–1140Q&T 650°C690–855
AISI 8630 Hardness (HV)Annealed145–180Normalized173–213Air Melted, Q&T220–270Q&T 205°C415–515Q&T 315°C385–475Q&T 425°C340–415Q&T 540°C280–345Q&T 650°C220–270

AISI 8630 Heat Treatment Key Points

The highest tensile strength is reached in the oil quenched & tempered at 205°C condition (1480–1810 MPa). The softest condition is annealed (145–180 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 205°C to 650°C lowers hardness from 415–515 HV to 220–270 HV, trading strength for toughness and ductility.

AISI 8630 Material Data Sheets

AISI 8630 Annealed | AISI 8630 Normalized | AISI 8630 Air Melted, Quenched & Tempered | AISI 8630 Oil Quenched & Tempered at 205°C | AISI 8630 Oil Quenched & Tempered at 315°C | AISI 8630 Oil Quenched & Tempered at 425°C | AISI 8630 Oil Quenched & Tempered at 540°C | AISI 8630 Oil Quenched & Tempered at 650°C | All AISI 8630 conditions

Looking for AISI 8630 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 8630 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.