AISI 8630 Air Melted, Quenched & Tempered Material Data Sheet

AISI 8630 Air Melted, Quenched & Tempered Material Data Sheet

AISI 8630 Air Melted, Quenched & Tempered Overview

AISI 8630 quenched tempered is AISI 8630 low alloy steel (UNS G86300, EN 30NiCrMo2-2) in the air melted, quenched & tempered condition. This AISI 8630 quenched tempered material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 8630 conditions in our AISI 8630 yield, tensile and hardness comparison. Looking for AISI 8630 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 8630 steel parts in-house and inspects them before shipment.

AISI 8630 Air Melted, Quenched & Tempered Designation

AISI 8630
ConditionQuenched & tempered
UNS numberG86300
US nameAMS 6535, AMS 6282, AMS 6357
EN name30NiCrMo2-2
EN number1.6545

AISI 8630 Air Melted, Quenched & Tempered Typical uses

General construction, general mechanical engineering, automotive, pressure vessels, pipework

AISI 8630 Air Melted, Quenched & Tempered Composition detail

C (carbon)0.28–0.33%
Cr (chromium)0.4–0.6%
Fe (iron)96.8–97.9%
Mn (manganese)0.7–0.9%
Mo (molybdenum)0.15–0.25%
Ni (nickel)0.4–0.7%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 8630 Air Melted, Quenched & Tempered Physical properties

Density7.79–7.87g/cm3

AISI 8630 Air Melted, Quenched & Tempered Mechanical properties

Young’s modulus200–210GPa
Specific stiffness25.5–26.9MN.m/kg
Yield strength (elastic limit)690–763MPa
Tensile strength862–953MPa
Specific strength88.1–97.4kN.m/kg
Elongation17–19.8% strain
Compressive strength752–831MPa
Flexural modulus200–210GPa
Flexural strength (modulus of rupture)690–763MPa
Shear modulus76–79.9GPa
Bulk modulus185–195GPa
Poisson’s ratio0.32–0.333 
Shape factor34
Hardness – Vickers220–270HV
Elastic stored energy (springs)1160–1420kJ/m3
Fatigue strength at 10^7 cycles330–384MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
315–402MPa

AISI 8630 Air Melted, Quenched & Tempered Impact & fracture properties

Fracture toughness47–77MPa.m0.5
Toughness (G)11.3–27.5kJ/m2

AISI 8630 Air Melted, Quenched & Tempered Thermal properties

Melting point1460–1510°C
Maximum service temperature445–496°C
Minimum service temperature-68–-43°C
Thermal conductivity42–45.5W/m.°C
Specific heat capacity461–480J/kg.°C
Thermal expansion coefficient12.4–13.1µstrain/°C
Thermal shock resistance261–295°C
Thermal distortion resistance3.28–3.6MW/m
Latent heat of fusion265–280kJ/kg

AISI 8630 Air Melted, Quenched & Tempered Electrical properties

Electrical resistivity23–35µohm.cm
Electrical conductivity4.93–7.5%IACS
Galvanic potential-0.51–-0.43V

AISI 8630 Air Melted, Quenched & Tempered Magnetic properties

Magnetic typeMagnetic

AISI 8630 Air Melted, Quenched & Tempered Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5050–5180m/s
Mechanical loss coefficient (tan delta)2e-4–6e-4 

AISI 8630 Air Melted, Quenched & Tempered Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed19.2 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.533 – 0.697

AISI 8630 Air Melted, Quenched & Tempered Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 8630 Air Melted, Quenched & Tempered Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 8630 Air Melted, Quenched & Tempered Notes

AISI 8630 Air Melted, Quenched & Tempered Warning
Some rare heat treatments of certain alloys may produce values for mechanical properties outside the given ranges, e.g. AISI 9255. tempered at 205C

AISI 8630 Air Melted, Quenched & Tempered Standards with similar compositions

Australia: 86B30H to AS 1444
France: 30NCD2 to AFNOR
Germany: 30NiCrMo2-2 to DIN
Italy: 30NiCrMo2KB to UNI 7356
Mexico: 8625 to NMX-B-203-SCFI, 8625 to NMX-B-300, 8627 to NMX-B-203-SCFI, 8627 to NMX-B-300, 8627H to NMX-B-268, 8627H to NMX-B-300, 8630 to NMX-B-203-SCFI, 8630 to NMX-B-300, 8630H to NMX-B-268, 8630H to NMX-B-300, 86B30H to NMX-B-300
Pan America: 8630 to COPANT 334
USA: 6535 to AMS 6535, 8625, 8625 to ASTM A29/A29M, 8625 to ASTM A331-95, 8625 to ASTM A519, 8625 to ASTM A829/A829M, 8625 to DoD-F-24669/1, 8625 to MIL-S-16974E, 8625 to SAE J404, 8625 to SAE J770, 8627, 8627 to ASTM A29/A29M, 8627 to ASTM A322-91, 8627 to ASTM A331-95, 8627 to ASTM A519, 8627 to ASTM A752/A752M, 8627 to ASTM A829/A829M, 8627 to DoD-F-24669/1, 8627 to SAE J404, 8627 to SAE J770, 8627H, 8630, 8630 to ASTM A29/A29M, 8630 to ASTM A322-91, 8630 to ASTM A331-95, 8630 to ASTM A513, 8630 to ASTM A519, 8630 to ASTM A752/A752M, 8630 to ASTM A829/A829M, 8630 to MIL-S-18728D, 8630 to SAE J404, 8630H, 8630H to ASTM A304, 8630H to ASTM A331-95, 8630H to SAE J1268, 8632, 86B30H, 86B30H to ASTM A304, 86B30H to ASTM A331-95, 86B30H to SAE J1268, EX 8, G86300 to ASTM A1031, G86300 to MIL-S-46059, UNS G86250, UNS G86270, UNS G86300, UNS H86270, UNS H86300, UNS H86301, UNS K13048, UNS K13049
Tradenames: KRUPP 30 NICRMO 2 2, SAARSTAHL 30 NICRMO 22, VB-30