AISI 8630 Normalized Material Data Sheet
AISI 8630 Normalized Overview
| AISI 8630 normalized is AISI 8630 low alloy steel (UNS G86300, EN 30NiCrMo2-2) in the normalized condition. This AISI 8630 normalized material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 8630 conditions in our AISI 8630 yield, tensile and hardness comparison. Looking for AISI 8630 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 8630 steel parts in-house and inspects them before shipment. |
AISI 8630 Normalized Designation
| AISI 8630 | |
| Condition | Normalized |
| UNS number | G86300 |
| US name | AMS 6535, AMS 6282, AMS 6357 |
| EN name | 30NiCrMo2-2 |
| EN number | 1.6545 |
AISI 8630 Normalized Typical uses
| General construction, general mechanical engineering, automotive, pressure vessels, pipework |
AISI 8630 Normalized Composition detail
| C (carbon) | 0.28 | – | 0.33 | % |
| Cr (chromium) | 0.4 | – | 0.6 | % |
| Fe (iron) | 96.8 | – | 97.9 | % |
| Mn (manganese) | 0.7 | – | 0.9 | % |
| Mo (molybdenum) | 0.15 | – | 0.25 | % |
| Ni (nickel) | 0.4 | – | 0.7 | % |
| P (phosphorus) | 0 | – | 0.035 | % |
| S (sulfur) | 0 | – | 0.04 | % |
| Si (silicon) | 0.15 | – | 0.35 | % |
AISI 8630 Normalized Physical properties
| Density | 7.79 | – | 7.87 | g/cm3 |
AISI 8630 Normalized Mechanical properties
| Young’s modulus | 200 | – | 210 | GPa |
| Specific stiffness | 25.5 | – | 26.9 | MN.m/kg |
| Yield strength (elastic limit) | 483 | – | 534 | MPa |
| Tensile strength | 621 | – | 686 | MPa |
| Specific strength | 61.7 | – | 68.2 | kN.m/kg |
| Elongation | 6 | – | 15 | % strain |
| Compressive strength | 483 | – | 534 | MPa |
| Flexural modulus | 200 | – | 210 | GPa |
| Flexural strength (modulus of rupture) | 483 | – | 534 | MPa |
| Shear modulus | 76 | – | 79.9 | GPa |
| Bulk modulus | 185 | – | 195 | GPa |
| Poisson’s ratio | 0.32 | – | 0.333 | |
| Shape factor | 46 | |||
| Hardness – Vickers | 173 | – | 213 | HV |
| Elastic stored energy (springs) | 569 | – | 695 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 294 | – | 339 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 277 | – | 360 | MPa |
AISI 8630 Normalized Impact & fracture properties
| Fracture toughness | 72 | – | 114 | MPa.m0.5 |
| Toughness (G) | 26.4 | – | 60.7 | kJ/m2 |
AISI 8630 Normalized Thermal properties
| Melting point | 1460 | – | 1510 | °C |
| Maximum service temperature | 445 | – | 496 | °C |
| Minimum service temperature | -73 | – | -48 | °C |
| Thermal conductivity | 47 | – | 50.9 | W/m.°C |
| Specific heat capacity | 461 | – | 480 | J/kg.°C |
| Thermal expansion coefficient | 12.4 | – | 13.1 | µstrain/°C |
| Thermal shock resistance | 183 | – | 207 | °C |
| Thermal distortion resistance | 3.67 | – | 4.03 | MW/m |
| Latent heat of fusion | 265 | – | 280 | kJ/kg |
AISI 8630 Normalized Electrical properties
| Electrical resistivity | 23 | – | 35 | µohm.cm |
| Electrical conductivity | 4.93 | – | 7.5 | %IACS |
| Galvanic potential | -0.51 | – | -0.43 | V |
AISI 8630 Normalized Magnetic properties
| Magnetic type | Magnetic |
AISI 8630 Normalized Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5050 | – | 5180 | m/s |
| Mechanical loss coefficient (tan delta) | 7.2e-4 | – | 8.9e-4 | |
AISI 8630 Normalized Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Excellent |
| Metal hot forming | Excellent |
| Metal press forming | Excellent |
| Metal deep drawing | Limited use |
| Machining speed | 25.6 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Good |
| Carbon equivalency | 0.533 – 0.697 |
AISI 8630 Normalized Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) | Acceptable |
| Flammability | Non-flammable |
AISI 8630 Normalized Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments | Slightly susceptible |
AISI 8630 Normalized Notes
| AISI 8630 Normalized Warning |
| Some rare heat treatments of certain alloys may produce values for mechanical properties outside the given ranges, e.g. AISI 9255. tempered at 205C |
AISI 8630 Normalized Standards with similar compositions
| Australia: 86B30H to AS 1444 |
| France: 30NCD2 to AFNOR |
| Germany: 30NiCrMo2-2 to DIN |
| Italy: 30NiCrMo2KB to UNI 7356 |
| Mexico: 8625 to NMX-B-203-SCFI, 8625 to NMX-B-300, 8627 to NMX-B-203-SCFI, 8627 to NMX-B-300, 8627H to NMX-B-268, 8627H to NMX-B-300, 8630 to NMX-B-203-SCFI, 8630 to NMX-B-300, 8630H to NMX-B-268, 8630H to NMX-B-300, 86B30H to NMX-B-300 |
| Pan America: 8630 to COPANT 334 |
| USA: 6535 to AMS 6535, 8625, 8625 to ASTM A29/A29M, 8625 to ASTM A331-95, 8625 to ASTM A519, 8625 to ASTM A829/A829M, 8625 to DoD-F-24669/1, 8625 to MIL-S-16974E, 8625 to SAE J404, 8625 to SAE J770, 8627, 8627 to ASTM A29/A29M, 8627 to ASTM A322-91, 8627 to ASTM A331-95, 8627 to ASTM A519, 8627 to ASTM A752/A752M, 8627 to ASTM A829/A829M, 8627 to DoD-F-24669/1, 8627 to SAE J404, 8627 to SAE J770, 8627H, 8630, 8630 to ASTM A29/A29M, 8630 to ASTM A322-91, 8630 to ASTM A331-95, 8630 to ASTM A513, 8630 to ASTM A519, 8630 to ASTM A752/A752M, 8630 to ASTM A829/A829M, 8630 to MIL-S-18728D, 8630 to SAE J404, 8630H, 8630H to ASTM A304, 8630H to ASTM A331-95, 8630H to SAE J1268, 8632, 86B30H, 86B30H to ASTM A304, 86B30H to ASTM A331-95, 86B30H to SAE J1268, EX 8, G86300 to ASTM A1031, G86300 to MIL-S-46059, UNS G86250, UNS G86270, UNS G86300, UNS H86270, UNS H86300, UNS H86301, UNS K13048, UNS K13049 |
| Tradenames: KRUPP 30 NICRMO 2 2, SAARSTAHL 30 NICRMO 22, VB-30 |