AISI 81B45 Tempering Temperature Comparison (205–650°C): Yield, Tensile & Hardness

How do the AISI 81B45 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 81B45 (UNS G81451) side by side for 5 conditions: Oil Quenched & Tempered at 205°C, Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 81B45 material data sheets linked below.

AISI 81B45 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Oil Quenched & Tempered at 205°C1550–19001830–2240495–6058–12
Oil Quenched & Tempered at 315°C1410–17301590–1950425–5256–10
Oil Quenched & Tempered at 425°C1180–14401270–1550363–4488.5–13.5
Oil Quenched & Tempered at 540°C920–1140990–1220305–37512.5–19.5
Oil Quenched & Tempered at 650°C710–875805–990255–31516–24

AISI 81B45 Differences Compared with Oil Quenched & Tempered at 205°C

The table below shows how much each condition differs from the oil quenched & tempered at 205°C condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Oil Quenched & Tempered at 315°C-9%-13%-14%-20%
Oil Quenched & Tempered at 425°C-24%-31%-26%+10%
Oil Quenched & Tempered at 540°C-40%-46%-38%+60%
Oil Quenched & Tempered at 650°C-54%-56%-48%+100%

AISI 81B45 Strength and Hardness Charts

AISI 81B45 Yield strength (MPa)Q&T 205°C1550–1900Q&T 315°C1410–1730Q&T 425°C1180–1440Q&T 540°C920–1140Q&T 650°C710–875
AISI 81B45 Tensile strength (MPa)Q&T 205°C1830–2240Q&T 315°C1590–1950Q&T 425°C1270–1550Q&T 540°C990–1220Q&T 650°C805–990
AISI 81B45 Hardness (HV)Q&T 205°C495–605Q&T 315°C425–525Q&T 425°C363–448Q&T 540°C305–375Q&T 650°C255–315

AISI 81B45 Heat Treatment Key Points

The highest tensile strength is reached in the oil quenched & tempered at 205°C condition (1830–2240 MPa). The softest condition is oil quenched & tempered at 650°C (255–315 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 205°C to 650°C lowers hardness from 495–605 HV to 255–315 HV, trading strength for toughness and ductility.

AISI 81B45 Material Data Sheets

AISI 81B45 Oil Quenched & Tempered at 205°C | AISI 81B45 Oil Quenched & Tempered at 315°C | AISI 81B45 Oil Quenched & Tempered at 425°C | AISI 81B45 Oil Quenched & Tempered at 540°C | AISI 81B45 Oil Quenched & Tempered at 650°C | All AISI 81B45 conditions