AISI 5140 Annealed vs Normalized vs Quenched & Tempered (205–650°C): Yield, Tensile & Hardness Compared

How do the AISI 5140 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 5140 (UNS G51400, EN 41Cr4) side by side for 7 conditions: Annealed, Normalized, Oil Quenched & Tempered at 205°C, Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 5140 material data sheets linked below.

AISI 5140 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Annealed260–325510–635155–19023–35
Normalized420–525710–875210–26018–28
Oil Quenched & Tempered at 205°C1480–18101610–1980440–5407–11
Oil Quenched & Tempered at 315°C1300–16001420–1740405–4958–12
Oil Quenched & Tempered at 425°C1050–13001180–1440330–40510–16
Oil Quenched & Tempered at 540°C770–955900–1100255–31513–21
Oil Quenched & Tempered at 650°C600–725675–840215–26520–30

AISI 5140 Differences Compared with Annealed

The table below shows how much each condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Normalized+62%+38%+36%-21%
Oil Quenched & Tempered at 205°C+462%+214%+184%-69%
Oil Quenched & Tempered at 315°C+396%+176%+161%-66%
Oil Quenched & Tempered at 425°C+302%+129%+113%-55%
Oil Quenched & Tempered at 540°C+195%+75%+65%-41%
Oil Quenched & Tempered at 650°C+126%+32%+39%-14%

AISI 5140 Strength and Hardness Charts

AISI 5140 Yield strength (MPa)Annealed260–325Normalized420–525Q&T 205°C1480–1810Q&T 315°C1300–1600Q&T 425°C1050–1300Q&T 540°C770–955Q&T 650°C600–725
AISI 5140 Tensile strength (MPa)Annealed510–635Normalized710–875Q&T 205°C1610–1980Q&T 315°C1420–1740Q&T 425°C1180–1440Q&T 540°C900–1100Q&T 650°C675–840
AISI 5140 Hardness (HV)Annealed155–190Normalized210–260Q&T 205°C440–540Q&T 315°C405–495Q&T 425°C330–405Q&T 540°C255–315Q&T 650°C215–265

AISI 5140 Heat Treatment Key Points

The highest tensile strength is reached in the oil quenched & tempered at 205°C condition (1610–1980 MPa). The softest condition is annealed (155–190 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 205°C to 650°C lowers hardness from 440–540 HV to 215–265 HV, trading strength for toughness and ductility.

AISI 5140 Material Data Sheets

AISI 5140 Annealed | AISI 5140 Normalized | AISI 5140 Oil Quenched & Tempered at 205°C | AISI 5140 Oil Quenched & Tempered at 315°C | AISI 5140 Oil Quenched & Tempered at 425°C | AISI 5140 Oil Quenched & Tempered at 540°C | AISI 5140 Oil Quenched & Tempered at 650°C | All AISI 5140 conditions

Looking for AISI 5140 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 5140 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.