How do the AISI 5130 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 5130 (UNS G51300, EN 34Cr4) side by side for 5 conditions: Oil Quenched & Tempered at 205°C, Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 5130 material data sheets linked below.

AISI 5130 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Oil Quenched & Tempered at 205°C1370–16701460–1780425–5258–12
Oil Quenched & Tempered at 315°C1270–15501350–1650395–4858–12
Oil Quenched & Tempered at 425°C1090–13301150–1410340–4209–15
Oil Quenched & Tempered at 540°C840–1040925–1140280–34012–18
Oil Quenched & Tempered at 650°C620–760710–875225–27516–24

AISI 5130 Differences Compared with Oil Quenched & Tempered at 205°C

The table below shows how much each condition differs from the oil quenched & tempered at 205°C condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Oil Quenched & Tempered at 315°C-7%-7%-7%+0%
Oil Quenched & Tempered at 425°C-20%-21%-20%+20%
Oil Quenched & Tempered at 540°C-38%-36%-35%+50%
Oil Quenched & Tempered at 650°C-55%-51%-47%+100%

AISI 5130 Strength and Hardness Charts

AISI 5130 Yield strength (MPa)Q&T 205°C1370–1670Q&T 315°C1270–1550Q&T 425°C1090–1330Q&T 540°C840–1040Q&T 650°C620–760
AISI 5130 Tensile strength (MPa)Q&T 205°C1460–1780Q&T 315°C1350–1650Q&T 425°C1150–1410Q&T 540°C925–1140Q&T 650°C710–875
AISI 5130 Hardness (HV)Q&T 205°C425–525Q&T 315°C395–485Q&T 425°C340–420Q&T 540°C280–340Q&T 650°C225–275

AISI 5130 Heat Treatment Key Points

The highest tensile strength is reached in the oil quenched & tempered at 205°C condition (1460–1780 MPa). The softest condition is oil quenched & tempered at 650°C (225–275 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 205°C to 650°C lowers hardness from 425–525 HV to 225–275 HV, trading strength for toughness and ductility.

AISI 5130 Material Data Sheets

AISI 5130 Oil Quenched & Tempered at 205°C | AISI 5130 Oil Quenched & Tempered at 315°C | AISI 5130 Oil Quenched & Tempered at 425°C | AISI 5130 Oil Quenched & Tempered at 540°C | AISI 5130 Oil Quenched & Tempered at 650°C | All AISI 5130 conditions

Looking for AISI 5130 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 5130 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.