AISI 4037 Tempering Temperature Comparison (205–650°C): Yield, Tensile & Hardness

How do the AISI 4037 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 4037 (UNS G40370) side by side for 5 conditions: Oil Quenched & Tempered at 205°C, Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 4037 material data sheets linked below.

AISI 4037 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Oil Quenched & Tempered at 205°C680–840920–1140280–3454–8
Oil Quenched & Tempered at 315°C685–845855–1050270–33011–17
Oil Quenched & Tempered at 425°C660–800785–970248–30316–24
Oil Quenched & Tempered at 540°C595–715710–875225–27518–28
Oil Quenched & Tempered at 650°C375–465620–770203–24823–35

AISI 4037 Differences Compared with Oil Quenched & Tempered at 205°C

The table below shows how much each condition differs from the oil quenched & tempered at 205°C condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Oil Quenched & Tempered at 315°C+1%-8%-4%+133%
Oil Quenched & Tempered at 425°C-4%-15%-12%+233%
Oil Quenched & Tempered at 540°C-14%-23%-20%+283%
Oil Quenched & Tempered at 650°C-45%-33%-28%+383%

AISI 4037 Strength and Hardness Charts

AISI 4037 Yield strength (MPa)Q&T 205°C680–840Q&T 315°C685–845Q&T 425°C660–800Q&T 540°C595–715Q&T 650°C375–465
AISI 4037 Tensile strength (MPa)Q&T 205°C920–1140Q&T 315°C855–1050Q&T 425°C785–970Q&T 540°C710–875Q&T 650°C620–770
AISI 4037 Hardness (HV)Q&T 205°C280–345Q&T 315°C270–330Q&T 425°C248–303Q&T 540°C225–275Q&T 650°C203–248

AISI 4037 Heat Treatment Key Points

The highest tensile strength is reached in the oil quenched & tempered at 205°C condition (920–1140 MPa). The softest condition is oil quenched & tempered at 650°C (203–248 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 205°C to 650°C lowers hardness from 280–345 HV to 203–248 HV, trading strength for toughness and ductility.

AISI 4037 Material Data Sheets

AISI 4037 Oil Quenched & Tempered at 205°C | AISI 4037 Oil Quenched & Tempered at 315°C | AISI 4037 Oil Quenched & Tempered at 425°C | AISI 4037 Oil Quenched & Tempered at 540°C | AISI 4037 Oil Quenched & Tempered at 650°C | All AISI 4037 conditions

Looking for AISI 4037 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 4037 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.