300M (Low Carbon, Quenched & Tempered Material Data Sheet

300M (Low Carbon, Quenched & Tempered Material Data Sheet

300M (Low Carbon, Quenched & Tempered Overview

300M (low carbon quenched tempered is 300M low alloy steel (UNS K44220, EN 41SiNiCrMoV7-6) in the (low carbon, quenched & tempered condition. This 300M (low carbon quenched tempered material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all 300M conditions in our 300M yield, tensile and hardness comparison. Looking for 300M parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined 300M steel parts in-house and inspects them before shipment.

300M (Low Carbon, Quenched & Tempered Designation

0.40C 300M
ConditionQuenched & tempered
UNS numberK44220
US nameAMS 6417, 4340M, MIL-S-8844
EN nameBS S 155, 41SiNiCrMoV7-6
EN number1.6928

300M (Low Carbon, Quenched & Tempered Typical uses

General construction, general mechanical engineering, automotive, pressure vessels, pipework

300M (Low Carbon, Quenched & Tempered Composition detail

C (carbon)0.38–0.42%
Cr (chromium)0.7–0.95%
Fe (iron)93.4–94.8%
Mn (manganese)0.6–0.9%
Mo (molybdenum)0.3–0.45%
Ni (nickel)1.65–2%
P (phosphorus)0–0.01%
S (sulfur)0–0.01%
Si (silicon)1.5–1.8%
V (vanadium)0.05–0.1%

300M (Low Carbon, Quenched & Tempered Physical properties

Density7.79–7.87g/cm3

300M (Low Carbon, Quenched & Tempered Mechanical properties

Young’s modulus200–210GPa
Specific stiffness25.5–26.9MN.m/kg
Yield strength (elastic limit)1520–1680MPa
Tensile strength1860–2060MPa
Specific strength194–214kN.m/kg
Elongation8–9.3% strain
Compressive strength1630–1800MPa
Flexural modulus200–210GPa
Flexural strength (modulus of rupture)1520–1680MPa
Shear modulus76–79.9GPa
Bulk modulus185–195GPa
Poisson’s ratio0.32–0.333 
Shape factor14
Hardness – Vickers551–609HV
Elastic stored energy (springs)5610–6860kJ/m3
Fatigue strength at 10^7 cycles800–883MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
754–937MPa

300M (Low Carbon, Quenched & Tempered Impact & fracture properties

Fracture toughness49.4–57.1MPa.m0.5
Toughness (G)12–15.9kJ/m2

300M (Low Carbon, Quenched & Tempered Thermal properties

Melting point1430–1510°C
Maximum service temperature220–246°C
Minimum service temperature-73–-43°C
Thermal conductivity55–59.6W/m.°C
Specific heat capacity461–480J/kg.°C
Thermal expansion coefficient12.4–13.1µstrain/°C
Thermal shock resistance575–649°C
Thermal distortion resistance4.29–4.71MW/m
Latent heat of fusion265–280kJ/kg

300M (Low Carbon, Quenched & Tempered Electrical properties

Electrical resistivity18–27µohm.cm
Electrical conductivity6.39–9.58%IACS
Galvanic potential-0.49–-0.41V

300M (Low Carbon, Quenched & Tempered Magnetic properties

Magnetic typeMagnetic

300M (Low Carbon, Quenched & Tempered Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5050–5180m/s
Mechanical loss coefficient (tan delta)2e-4–5e-4 

300M (Low Carbon, Quenched & Tempered Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed7.01 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.8 – 1

300M (Low Carbon, Quenched & Tempered Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

300M (Low Carbon, Quenched & Tempered Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Susceptible

300M (Low Carbon, Quenched & Tempered Notes

300M (Low Carbon, Quenched & Tempered Warning
Some rare heat treatments of certain alloys may produce values for mechanical properties outside the given ranges, e.g. AISI 9255. tempered at 205C

300M (Low Carbon, Quenched & Tempered Standards with similar compositions

USA: 300M to SAE J467, 4340M to MIL-S-83135, Grade 8 to ASTM A646-95