300M (high carbon quenched tempered is 300M low alloy steel (UNS K44220, EN 41SiNiCrMoV7-6) in the (high carbon, quenched & tempered condition. This 300M (high carbon quenched tempered material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all 300M conditions in our 300M yield, tensile and hardness comparison . Looking for 300M parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined 300M steel parts in-house and inspects them before shipment.
300M (High Carbon, Quenched & Tempered Designation
0.42C 300M Condition Quenched & tempered UNS number K44220 US name AMS 6419, 4340M, MIL-S-8844 EN name BS S 155, 41SiNiCrMoV7-6 EN number 1.6928
300M (High Carbon, Quenched & Tempered Typical uses
General construction, general mechanical engineering, automotive, pressure vessels, pipework
300M (High Carbon, Quenched & Tempered Composition detail
C (carbon) 0.4 – 0.44 % Cr (chromium) 0.7 – 0.95 % Fe (iron) 93.3 – 94.8 % Mn (manganese) 0.6 – 0.9 % Mo (molybdenum) 0.3 – 0.45 % Ni (nickel) 1.65 – 2 % P (phosphorus) 0 – 0.01 % S (sulfur) 0 – 0.01 % Si (silicon) 1.5 – 1.8 % V (vanadium) 0.05 – 0.1 %
300M (High Carbon, Quenched & Tempered Physical properties
300M (High Carbon, Quenched & Tempered Mechanical properties
Young’s modulus 200 – 210 GPa Specific stiffness 25.5 – 26.9 MN.m/kg Yield strength (elastic limit) 1590 – 1750 MPa Tensile strength 1930 – 2130 MPa Specific strength 202 – 224 kN.m/kg Elongation 7 – 8.14 % strain Compressive strength 1700 – 1880 MPa Flexural modulus 200 – 210 GPa Flexural strength (modulus of rupture) 1590 – 1750 MPa Shear modulus 76 – 79.9 GPa Bulk modulus 185 – 195 GPa Poisson’s ratio 0.32 – 0.333 Shape factor 14 Hardness – Vickers 551 – 609 HV Elastic stored energy (springs) 6130 – 7500 kJ/m3 Fatigue strength at 10^7 cycles 800 – 883 MPa Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles 754 – 936 MPa
300M (High Carbon, Quenched & Tempered Impact & fracture properties
Fracture toughness 49.4 – 57.1 MPa.m0.5 Toughness (G) 12 – 15.9 kJ/m2
300M (High Carbon, Quenched & Tempered Thermal properties
Melting point 1430 – 1510 °C Maximum service temperature 220 – 246 °C Minimum service temperature -73 – -43 °C Thermal conductivity 55 – 59.6 W/m.°C Specific heat capacity 461 – 480 J/kg.°C Thermal expansion coefficient 12.4 – 13.1 µstrain/°C Thermal shock resistance 601 – 678 °C Thermal distortion resistance 4.29 – 4.71 MW/m Latent heat of fusion 265 – 280 kJ/kg
300M (High Carbon, Quenched & Tempered Electrical properties
Electrical resistivity 18 – 27 µohm.cm Electrical conductivity 6.39 – 9.58 %IACS Galvanic potential -0.49 – -0.41 V
300M (High Carbon, Quenched & Tempered Magnetic properties
300M (High Carbon, Quenched & Tempered Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 5050 – 5180 m/s Mechanical loss coefficient (tan delta) 2e-4 – 5e-4
300M (High Carbon, Quenched & Tempered Processing properties
Metal casting Unsuitable Metal cold forming Excellent Metal hot forming Excellent Metal press forming Excellent Metal deep drawing Limited use Machining speed 7.01 m/min Weldability Notes: Preheating and post weld heat treatments are required Good Carbon equivalency 0.82 – 1.02
300M (High Carbon, Quenched & Tempered Durability
Water (fresh) Acceptable Water (salt) Limited use Weak acids Limited use Strong acids Unacceptable Weak alkalis Acceptable Strong alkalis Limited use Organic solvents Excellent Oxidation at 500C Acceptable UV radiation (sunlight) Excellent Galling resistance (adhesive wear) Acceptable Flammability Non-flammable
300M (High Carbon, Quenched & Tempered Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments Susceptible
300M (High Carbon, Quenched & Tempered Notes
300M (High Carbon, Quenched & Tempered Warning Some rare heat treatments of certain alloys may produce values for mechanical properties outside the given ranges, e.g. AISI 9255. tempered at 205C
300M (High Carbon, Quenched & Tempered Standards with similar compositions
UK: S-155A to BS S 155, S-155B to BS S 155, S-155C to BS S 155USA: 32 to ASTM A579, UNS K44220Tradenames: E 300M, KRUPP HFX 6928, TRICENT, VASCO 300M