AISI 9255 Oil Quenched & Tempered at 540°C Material Data Sheet

AISI 9255 Oil Quenched & Tempered at 540°C Material Data Sheet

AISI 9255 Oil Quenched & Tempered at 540°C Overview

AISI 9255 tempered 540°C is AISI 9255 low alloy steel (UNS G92550, EN 55Si7) in the oil quenched & tempered at 540°C condition. This AISI 9255 tempered 540°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 9255 conditions in our AISI 9255 yield, tensile and hardness comparison. Looking for AISI 9255 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 9255 steel parts in-house and inspects them before shipment.

AISI 9255 Oil Quenched & Tempered at 540°C Designation

AISI 9255
ConditionTempered at 540°C & oil quenched
UNS numberG92550
EN name55Si7, 56Si7, 251A58
EN number1.5026

AISI 9255 Oil Quenched & Tempered at 540°C Typical uses

Laminated springs, coil springs, torsion bars of heavy section

AISI 9255 Oil Quenched & Tempered at 540°C Composition detail

C (carbon)0.51–0.59%
Fe (iron)96.2–97%
Mn (manganese)0.7–0.95%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)1.8–2.2%

AISI 9255 Oil Quenched & Tempered at 540°C Physical properties

Density7.8–7.9g/cm3

AISI 9255 Oil Quenched & Tempered at 540°C Mechanical properties

Young’s modulus206–216GPa
Specific stiffness26.2–27.5MN.m/kg
Yield strength (elastic limit)990–1220MPa
Tensile strength1130–1380MPa
Specific strength126–155kN.m/kg
Elongation12–18% strain
Compressive strength990–1220MPa
Flexural modulus206–216GPa
Flexural strength (modulus of rupture)990–1220MPa
Shear modulus79–85GPa
Bulk modulus159–176GPa
Poisson’s ratio0.285–0.295 
Shape factor22
Hardness – Vickers318–393HV
Elastic stored energy (springs)2340–3470kJ/m3
Fatigue strength at 10^7 cycles466–537MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
408–613MPa

AISI 9255 Oil Quenched & Tempered at 540°C Impact & fracture properties

Fracture toughness38–66MPa.m0.5
Toughness (G)7.27–19.5kJ/m2

AISI 9255 Oil Quenched & Tempered at 540°C Thermal properties

Melting point1390–1500°C
Maximum service temperature500–530°C
Minimum service temperature-63–-33°C
Thermal conductivity46–51W/m.°C
Specific heat capacity425–475J/kg.°C
Thermal expansion coefficient11–13µstrain/°C
Thermal shock resistance381–496°C
Thermal distortion resistance3.68–4.46MW/m
Latent heat of fusion265–280kJ/kg

AISI 9255 Oil Quenched & Tempered at 540°C Electrical properties

Electrical resistivity15–35µohm.cm
Electrical conductivity4.93–11.5%IACS
Galvanic potential-0.51–-0.43V

AISI 9255 Oil Quenched & Tempered at 540°C Magnetic properties

Magnetic typeMagnetic

AISI 9255 Oil Quenched & Tempered at 540°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5120–5250m/s
Mechanical loss coefficient (tan delta)3.2e-4–4e-4 

AISI 9255 Oil Quenched & Tempered at 540°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed13.4 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.627 – 0.748

AISI 9255 Oil Quenched & Tempered at 540°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 9255 Oil Quenched & Tempered at 540°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 9255 Oil Quenched & Tempered at 540°C Notes

AISI 9255 Oil Quenched & Tempered at 540°C Other notes
A spring steel, used for more highly stressed applications than carbon steels.

AISI 9255 Oil Quenched & Tempered at 540°C Standards with similar compositions

Australia: 9255 to AS 1444
Belgium: 55Si7 to NBN 253-05
Germany: 1.0904 to DIN, 1.5026 to DIN 17222, 55Si7 to DIN 17222
Hungary: 55Si7 to MSZ 2666
India: 50Si7 to IS 4072, 50Si7 to IS 8055, 55Si2Mn90 to IS 4368, 55Si2Mo90 to IS 6967, 55Si7 to IS 1570/4, 55Si7 to IS 2507, 55Si7 to IS 3195, 55Si7 to IS 3431, 55Si7 to IS 3885/1, 55Si7 to IS 3885/2, 55Si7 to IS 4072, 55Si7 to IS 8052, 55Si7 to IS 8055, Grade 2 to IS 8051, Grade 3 to IS 9442
Italy: 56SiMn7KU to UNI 2955/3
Mexico: 9255 to NMX-B-203-SCFI, 9255 to NMX-B-300
Pan America: 9255 to COPANT 334, 9255 to COPANT 514
Serbia and Montenegro: C.2133
Spain: 56Si7 to UNE 36015, F.1440 to UNE 36015
Sweden: 2090 to SS 142090
UK: 250A53 to BS 970/1
USA: 9250, 9255, 9255 to ASTM A29/A29M, 9255 to ASTM A519, UNS G92550
Tradenames: 56 SI 7, A-144, A-145, AIREX, ALAIS AES8, AMBO MS 5, B.S.C. SI-MN, BOCHUMER NZF S/O, BOFORS S-145, BOHLER F110, BOHLER SMF, CHATILLON MN SI, DISQUE H, FAGERSTA FB-S4, FAGERSTA S310, FORTUNA GFD5W, HOFORS SM-5, MULTOLE, NASCOLOY O, POMPEY RS 2, POMPEY RS3, ROCHLING RFA, S.M. STEEL, SAARSTAHL 55 SI 7, SAUT-DU-TARN 55.S6, SILICO MANGANESE SPRING WIRE, SUWEFA GFD5W, SUWEFA SJII, TKS 55 SI 7, TOLEDO H-O SILICOMANGANESE, WEFAHUTTE HLSFW, WIKMANS VH-FS