AISI 8660 Oil Quenched & Tempered at 540°C Material Data Sheet
AISI 8660 Oil Quenched & Tempered at 540°C Material Data Sheet
AISI 8660 Oil Quenched & Tempered at 540°C Overview
AISI 8660 tempered 540°C is AISI 8660 low alloy steel (UNS G86600) in the oil quenched & tempered at 540°C condition. This AISI 8660 tempered 540°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 8660 conditions in our AISI 8660 yield, tensile and hardness comparison. Looking for AISI 8660 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 8660 steel parts in-house and inspects them before shipment.
AISI 8660 Oil Quenched & Tempered at 540°C Designation
AISI 8660 Oil Quenched & Tempered at 540°C Thermal properties
Melting point
1380
–
1490
°C
Maximum service temperature
500
–
530
°C
Minimum service temperature
-58
–
-33
°C
Thermal conductivity
34
–
44
W/m.°C
Specific heat capacity
460
–
500
J/kg.°C
Thermal expansion coefficient
11
–
13
µstrain/°C
Thermal shock resistance
429
–
557
°C
Thermal distortion resistance
2.78
–
3.76
MW/m
Latent heat of fusion
265
–
280
kJ/kg
AISI 8660 Oil Quenched & Tempered at 540°C Electrical properties
Electrical resistivity
23
–
35
µohm.cm
Electrical conductivity
4.93
–
7.5
%IACS
Galvanic potential
-0.5
–
-0.42
V
AISI 8660 Oil Quenched & Tempered at 540°C Magnetic properties
Magnetic type
Magnetic
AISI 8660 Oil Quenched & Tempered at 540°C Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5060
–
5200
m/s
Mechanical loss coefficient (tan delta)
3e-4
–
3.8e-4
AISI 8660 Oil Quenched & Tempered at 540°C Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
12.2 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Poor
Carbon equivalency
0.812 – 1.03
AISI 8660 Oil Quenched & Tempered at 540°C Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
AISI 8660 Oil Quenched & Tempered at 540°C Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible
AISI 8660 Oil Quenched & Tempered at 540°C Standards with similar compositions
Australia: 8660 to AS 1444, 8660H to AS 1444
Mexico: 8660 to NMX-B-203-SCFI, 8660 to NMX-B-300, 8660H to NMX-B-268, 8660H to NMX-B-300
Pan America: 8660 to COPANT 334, 8660 to COPANT 514
UK: 805A60 to BS 970/1, 805H60 to BS 970/1, 805H60 to BS 970/2
USA: 8660, 8660 to ASTM A29/A29M, 8660 to ASTM A519, 8660 to SAE J770, 8660H, 8660H to ASTM A304, 8660H to ASTM A331-95, 8660H to SAE J1268, G86600 to ASTM A1031, UNS G86600, UNS H86600