AISI 8640 Oil Quenched & Tempered at 650°C Material Data Sheet
AISI 8640 Oil Quenched & Tempered at 650°C Overview
| AISI 8640 tempered 650°C is AISI 8640 low alloy steel (UNS G86400) in the oil quenched & tempered at 650°C condition. This AISI 8640 tempered 650°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 8640 conditions in our AISI 8640 yield, tensile and hardness comparison. Looking for AISI 8640 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 8640 steel parts in-house and inspects them before shipment. |
AISI 8640 Oil Quenched & Tempered at 650°C Designation
| AISI 8640 | |
| Condition | Tempered at 650°C & oil quenched |
| UNS number | G86400 |
| US name | SAE 8740, ASTM 8640, ASTM G86400, ASTM 8740H, ASTM 8740, ASTM 8640H, ASTM 8640, ~SAE 8640, ~SAE 8640 |
| ISO name | 41 CrNiMoS 2, 41CrNiMoS2, 41CrNiMo2E, ~41CrNiMo2 |
| JIS (Japanese) name | SNCM240 |
AISI 8640 Oil Quenched & Tempered at 650°C Typical uses
| General construction, general mechanical engineering, automotive, tools, axles, gears, springs. |
AISI 8640 Oil Quenched & Tempered at 650°C Composition detail
| C (carbon) | 0.38 | – | 0.43 | % |
| Cr (chromium) | 0.4 | – | 0.6 | % |
| Fe (iron) | 96.6 | – | 97.8 | % |
| Mn (manganese) | 0.75 | – | 1 | % |
| Mo (molybdenum) | 0.15 | – | 0.25 | % |
| Ni (nickel) | 0.4 | – | 0.7 | % |
| P (phosphorus) | 0 | – | 0.035 | % |
| S (sulfur) | 0 | – | 0.04 | % |
| Si (silicon) | 0.15 | – | 0.35 | % |
AISI 8640 Oil Quenched & Tempered at 650°C Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 8640 Oil Quenched & Tempered at 650°C Mechanical properties
| Young’s modulus | 201 | – | 212 | GPa |
| Specific stiffness | 25.6 | – | 27 | MN.m/kg |
| Yield strength (elastic limit) | 720 | – | 880 | MPa |
| Tensile strength | 805 | – | 990 | MPa |
| Specific strength | 91.7 | – | 112 | kN.m/kg |
| Elongation | 16 | – | 24 | % strain |
| Compressive strength | 720 | – | 880 | MPa |
| Flexural modulus | 201 | – | 212 | GPa |
| Flexural strength (modulus of rupture) | 720 | – | 880 | MPa |
| Shear modulus | 77 | – | 83 | GPa |
| Bulk modulus | 155 | – | 173 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 31 | |||
| Hardness – Vickers | 255 | – | 315 | HV |
| Elastic stored energy (springs) | 1270 | – | 1860 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 367 | – | 426 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 320 | – | 489 | MPa |
AISI 8640 Oil Quenched & Tempered at 650°C Impact & fracture properties
| Fracture toughness | 45 | – | 74 | MPa.m0.5 |
| Toughness (G) | 10.3 | – | 25.3 | kJ/m2 |
AISI 8640 Oil Quenched & Tempered at 650°C Thermal properties
| Melting point | 1430 | – | 1510 | °C |
| Maximum service temperature | 610 | – | 640 | °C |
| Minimum service temperature | -68 | – | -43 | °C |
| Thermal conductivity | 36 | – | 46 | W/m.°C |
| Specific heat capacity | 460 | – | 500 | J/kg.°C |
| Thermal expansion coefficient | 10.5 | – | 13 | µstrain/°C |
| Thermal shock resistance | 285 | – | 382 | °C |
| Thermal distortion resistance | 2.97 | – | 4.08 | MW/m |
| Latent heat of fusion | 265 | – | 280 | kJ/kg |
AISI 8640 Oil Quenched & Tempered at 650°C Electrical properties
| Electrical resistivity | 23 | – | 35 | µohm.cm |
| Electrical conductivity | 4.93 | – | 7.5 | %IACS |
| Galvanic potential | -0.51 | – | -0.43 | V |
AISI 8640 Oil Quenched & Tempered at 650°C Magnetic properties
| Magnetic type | Magnetic |
AISI 8640 Oil Quenched & Tempered at 650°C Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5060 | – | 5200 | m/s |
| Mechanical loss coefficient (tan delta) | 4.4e-4 | – | 5.6e-4 | |
AISI 8640 Oil Quenched & Tempered at 650°C Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Excellent |
| Metal hot forming | Excellent |
| Metal press forming | Excellent |
| Metal deep drawing | Limited use |
| Machining speed | 17.4 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Good |
| Carbon equivalency | 0.642 – 0.813 |
AISI 8640 Oil Quenched & Tempered at 650°C Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) | Acceptable |
| Flammability | Non-flammable |
AISI 8640 Oil Quenched & Tempered at 650°C Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments | Slightly susceptible |
AISI 8640 Oil Quenched & Tempered at 650°C Standards with similar compositions
| Argentina: IRAM 8640 to IAS |
| Australia: 8640 to AS 1444 |
| Hungary: NCMo3 to MSZ 61, NCMo3Z to MSZ 6251 |
| International: 41CrNiMo2E to ISO 4954 |
| Italy: 40NiCrMo2 to UNI 7845 |
| Japan: SNCM 240 to JIS G4053 |
| Mexico: 8637 to NMX-B-203-SCFI, 8637 to NMX-B-300, 8637H to NMX-B-268, 8637H to NMX-B-300, 8640 to NMX-B-203-SCFI, 8640 to NMX-B-300, 8640H to NMX-B-268, 8640H to NMX-B-300, 8642 to NMX-B-300, 8642H to NMX-B-268, 8642H to NMX-B-300 |
| Pan America: 8637 to COPANT 334, 8640 to COPANT 334 |
| Poland: 37HGNM to PN-H-84030, 37HGNM to PN-H-84030/04 |
| USA: 8637, 8637 to ASTM A29/A29M, 8637 to ASTM A322-91, 8637 to ASTM A331-95, 8637 to ASTM A519, 8637 to ASTM A752/A752M, 8637 to ASTM A829/A829M, 8637 to SAE J770, 8637H, 8637H to ASTM A304, 8637H to ASTM A331-95, 8637H to SAE J1268, 8640, 8640 to ASTM A29/A29M, 8640 to ASTM A322-91, 8640 to ASTM A331-95, 8640 to ASTM A519, 8640 to ASTM A752/A752M, 8640 to ASTM A829/A829M, 8640 to SAE J404, 8640H, 8640H to ASTM A304, 8640H to ASTM A331-95, 8640H to SAE J1268, 8642, 8642 to ASTM A29/A29M, 8642 to ASTM A322-91, 8642 to ASTM A331-95, 8642 to ASTM A519, 8642 to ASTM A752/A752M, 8642H, 8642H to ASTM A304, 8642H to ASTM A331-95, 8642H to SAE J1268, 94B40, 94B40 to ASTM A519, G86400 to ASTM A1031, G86420 to ASTM A1031, UNS G86370, UNS G86400, UNS G86420, UNS G94401, UNS H86370, UNS H86400, UNS H86420 |
| Tradenames: DF 40 NI CR MO 2, HEVA-DF-120, MONIX 40, VB-40 |