AISI 6150 Oil Quenched & Tempered at 540°C Material Data Sheet

AISI 6150 Oil Quenched & Tempered at 540°C Material Data Sheet

AISI 6150 Oil Quenched & Tempered at 540°C Overview

AISI 6150 tempered 540°C is AISI 6150 low alloy steel (UNS G61500, EN 51CrMnV4) in the oil quenched & tempered at 540°C condition. This AISI 6150 tempered 540°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 6150 conditions in our AISI 6150 yield, tensile and hardness comparison. Looking for AISI 6150 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 6150 steel parts in-house and inspects them before shipment.

AISI 6150 Oil Quenched & Tempered at 540°C Designation

AISI 6150
ConditionTempered at 540°C & oil quenched
UNS numberG61500, H61500, K15048, K15047
US nameASTM A231, ASTM A232, ASTM A646 Grade 14
EN name735A50, BS S 204, 51CrMnV4
EN number1.8158, 1.8159, 1.2241
ISO name51CrV6, 51CrV4

AISI 6150 Oil Quenched & Tempered at 540°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 6150 Oil Quenched & Tempered at 540°C Composition detail

C (carbon)0.48–0.53%
Cr (chromium)0.8–1.1%
Fe (iron)96.9–97.7%
Mn (manganese)0.7–0.9%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%
V (vanadium)0.15  %

AISI 6150 Oil Quenched & Tempered at 540°C Physical properties

Density7.8–7.9g/cm3

AISI 6150 Oil Quenched & Tempered at 540°C Mechanical properties

Young’s modulus201–212GPa
Specific stiffness25.6–27MN.m/kg
Yield strength (elastic limit)960–1180MPa
Tensile strength1040–1280MPa
Specific strength122–150kN.m/kg
Elongation10–16% strain
Compressive strength960–1180MPa
Flexural modulus201–212GPa
Flexural strength (modulus of rupture)960–1180MPa
Shear modulus77–83GPa
Bulk modulus155–173GPa
Poisson’s ratio0.285–0.295 
Shape factor22
Hardness – Vickers310–380HV
Elastic stored energy (springs)2250–3340kJ/m3
Fatigue strength at 10^7 cycles439–508MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
384–581MPa

AISI 6150 Oil Quenched & Tempered at 540°C Impact & fracture properties

Fracture toughness37–64MPa.m0.5
Toughness (G)7.03–18.7kJ/m2

AISI 6150 Oil Quenched & Tempered at 540°C Thermal properties

Melting point1410–1500°C
Maximum service temperature500–530°C
Minimum service temperature-63–-38°C
Thermal conductivity35–55W/m.°C
Specific heat capacity420–520J/kg.°C
Thermal expansion coefficient11.5–13µstrain/°C
Thermal shock resistance374–476°C
Thermal distortion resistance2.84–4.53MW/m
Latent heat of fusion265–280kJ/kg

AISI 6150 Oil Quenched & Tempered at 540°C Electrical properties

Electrical resistivity15–30µohm.cm
Electrical conductivity5.75–11.5%IACS
Galvanic potential-0.5–-0.42V

AISI 6150 Oil Quenched & Tempered at 540°C Magnetic properties

Magnetic typeMagnetic

AISI 6150 Oil Quenched & Tempered at 540°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5060–5200m/s
Mechanical loss coefficient (tan delta)3.4e-4–4.3e-4 

AISI 6150 Oil Quenched & Tempered at 540°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed14 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.787 – 0.93

AISI 6150 Oil Quenched & Tempered at 540°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 6150 Oil Quenched & Tempered at 540°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 6150 Oil Quenched & Tempered at 540°C Standards with similar compositions

Australia: 6150 to AS 1444, 6150H to AS 1444
Belgium: 50CrV4 to NBN 253-02, 50CrV4 to NBN 253-05
France: 50CV4 to AFNOR NF A35-552, 50CV4 to AFNOR NF A35-553, 50CV4 to AFNOR NF A35-571
Germany: 1.2241 to DIN 17350, 1.8159 to DIN 1652, 1.8159 to DIN 17221, 1.8159 to DIN EN 10083, 50CrV4 to DIN EN 10083, 51CrMnV4 to DIN 17350
Hungary: 50CV2 to MSZ 4217, 51CrV4 to MSZ 2666, CrV3 to MSZ 61, CrV3E to MSZ 61, CrV3Z to MSZ 6251
India: 50Cr1V23 to IS 4368, 50Cr4V1 to IS 13352, 50Cr4V2 to IS 11185, 50Cr4V2 to IS 2507, 50Cr4V2 to IS 3885/2, 50Cr4V2 to IS 3930, 50Cr4V2 to IS 7494, 50Cr4V2 to IS 8052, 50CrV4 to IS 4072, 50CrV4 to IS 8055, FDCrV-A to IS 4454/2, TDCrV-A to IS 4454/2, VDCrV-A to IS 4454/2
International: 51CrV4 to ISO 683-1, 51CrV4 to ISO 683-14, 51CrV6 to ISO 683-18, FDCrV-A to ISO 8458-3, TDCrV-A to ISO 8458-3, VDCrV-A to ISO 8458-3
Italy: 50CrV4 to UNI 3545, 50CrV4 to UNI 7064, 50CrV4 to UNI 7065, 50CrV4 to UNI 7845, 50CrV4 to UNI 7874, 50CrV4 to UNI 8893, 51CrMnV4KU to UNI 2955/3, 51CrV3KU to UNI 2955
Japan: SWOCV-V to JIS G3561
Mexico: 6150 to NMX-B-203-SCFI, 6150 to NMX-B-300, 6150H to NMX-B-268, 6150H to NMX-B-300
Pan America: 6150 to COPANT 334
Romania: 50VCr11 to STAS 791, 50VCr11CS to STAS 10677, 51VMnCr11 to STAS 791, 51VMnCr11S to STAS 791, 51VMnCr11X to STAS 791, 51VMnCr11XS to STAS 791
Serbia and Montenegro: C.4830
South Korea: SPS 6 to KS D 3701
Spain: 51CrV4 to UNE 36015, F.1430 to UNE 36015
Turkey: 50CrV4-1,8159 to TS 2288
UK: 51CrV4 to BS EN 10083-1, 51CrV4 to BS EN 10250-3, 51CrV4 to BS EN 10277-5, 735A50 to BS 1429, 735A50 to BS 970/1, 735A51 to BS 970/2, 735H51 to BS 970/2
USA: 6145, 6150, 6150 to ASTM A29/A29M, 6150 to ASTM A519, 6150 to ASTM A829/A829M, 6150 to MIL-S-8503, 6150 to SAE J404, A231 to ASTM A231/A231M, A232 to ASTM A232/A232M, G61500 to ASTM A1031, Grade 14 to ASTM A646-95, UNS G61500, UNS H61500, UNS K15047, UNS K15048
Tradenames: 50 CR V 4, A-143, ACENOR MCV, AMBO FAW, ASCOMETAL 50CV4, BERGISCHE 50 CMV, CYCLOPS L2, DIRO-50 CRV 4, FORTUNA TCV4, GDH-L2, JESSOP ET NO. 6, KRUPP WL 1.8154, PLATE PN 24, SAARSTAHL 50 CRV 4, SHARON 6100 SERIES B, TKS 50 CRV 4, VERTOMAR CV50, VL3, VN-50, WEINGARTNER EW 8159, WESTIG 50 CR V 4, WITTEN PCVWL