AISI 51B60 Oil Quenched & Tempered at 540°C Material Data Sheet

AISI 51B60 Oil Quenched & Tempered at 540°C Material Data Sheet

AISI 51B60 Oil Quenched & Tempered at 540°C Overview

AISI 51B60 tempered 540°C is AISI 51B60 low alloy steel (UNS G51601) in the oil quenched & tempered at 540°C condition. This AISI 51B60 tempered 540°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 51B60 conditions in our AISI 51B60 yield, tensile and hardness comparison. Looking for AISI 51B60 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 51B60 steel parts in-house and inspects them before shipment.

AISI 51B60 Oil Quenched & Tempered at 540°C Designation

AISI 51B60
ConditionTempered at 540°C & oil quenched
UNS numberG51601
US nameASTM 51B60, ~ASTM 50B60, ~ASTM 51B60

AISI 51B60 Oil Quenched & Tempered at 540°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 51B60 Oil Quenched & Tempered at 540°C Composition detail

B (boron)5e-4–0.003%
C (carbon)0.56–0.64%
Cr (chromium)0.7–0.9%
Fe (iron)97–97.8%
Mn (manganese)0.75–1%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 51B60 Oil Quenched & Tempered at 540°C Physical properties

Density7.8–7.9g/cm3

AISI 51B60 Oil Quenched & Tempered at 540°C Mechanical properties

Young’s modulus201–212GPa
Specific stiffness25.6–27MN.m/kg
Yield strength (elastic limit)990–1220MPa
Tensile strength1080–1310MPa
Specific strength126–155kN.m/kg
Elongation12–18% strain
Compressive strength990–1220MPa
Flexural modulus201–212GPa
Flexural strength (modulus of rupture)990–1220MPa
Shear modulus77–83GPa
Bulk modulus155–173GPa
Poisson’s ratio0.285–0.295 
Shape factor22
Hardness – Vickers320–395HV
Elastic stored energy (springs)2390–3550kJ/m3
Fatigue strength at 10^7 cycles451–518MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
397–589MPa

AISI 51B60 Oil Quenched & Tempered at 540°C Impact & fracture properties

Fracture toughness37–63MPa.m0.5
Toughness (G)7.01–18.2kJ/m2

AISI 51B60 Oil Quenched & Tempered at 540°C Thermal properties

Melting point1380–1490°C
Maximum service temperature500–530°C
Minimum service temperature-63–-33°C
Thermal conductivity41–48W/m.°C
Specific heat capacity440–520J/kg.°C
Thermal expansion coefficient11.5–13µstrain/°C
Thermal shock resistance385–490°C
Thermal distortion resistance3.29–4MW/m
Latent heat of fusion265–280kJ/kg

AISI 51B60 Oil Quenched & Tempered at 540°C Electrical properties

Electrical resistivity22–30µohm.cm
Electrical conductivity5.75–7.84%IACS
Galvanic potential-0.5–-0.42V

AISI 51B60 Oil Quenched & Tempered at 540°C Magnetic properties

Magnetic typeMagnetic

AISI 51B60 Oil Quenched & Tempered at 540°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5060–5200m/s
Mechanical loss coefficient (tan delta)3.3e-4–4.1e-4 

AISI 51B60 Oil Quenched & Tempered at 540°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed13.4 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Poor
Carbon equivalency0.825 – 0.987

AISI 51B60 Oil Quenched & Tempered at 540°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 51B60 Oil Quenched & Tempered at 540°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 51B60 Oil Quenched & Tempered at 540°C Standards with similar compositions

China: 60CrMnBA to GB 1222
Pan America: 51B60 to COPANT 514
USA: 51B60, 51B60 to ASTM A29/A29M, 51B60 to ASTM A322-91, 51B60 to SAE J770, 51B60H, 51B60H to ASTM A304, 51B60H to SAE J1268, UNS H51601