AISI 51B60 Oil Quenched & Tempered at 650°C Material Data Sheet
AISI 51B60 Oil Quenched & Tempered at 650°C Material Data Sheet
AISI 51B60 Oil Quenched & Tempered at 650°C Overview
AISI 51B60 tempered 650°C is AISI 51B60 low alloy steel (UNS G51601) in the oil quenched & tempered at 650°C condition. This AISI 51B60 tempered 650°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 51B60 conditions in our AISI 51B60 yield, tensile and hardness comparison. Looking for AISI 51B60 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 51B60 steel parts in-house and inspects them before shipment.
AISI 51B60 Oil Quenched & Tempered at 650°C Designation
AISI 51B60
Condition
Tempered at 650°C & oil quenched
UNS number
G51601
US name
ASTM 51B60, ~ASTM 50B60, ~ASTM 51B60
AISI 51B60 Oil Quenched & Tempered at 650°C Typical uses
General construction, general mechanical engineering, automotive, tools, axles, gears, springs.
AISI 51B60 Oil Quenched & Tempered at 650°C Composition detail
B (boron)
5e-4
–
0.003
%
C (carbon)
0.56
–
0.64
%
Cr (chromium)
0.7
–
0.9
%
Fe (iron)
97
–
97.8
%
Mn (manganese)
0.75
–
1
%
P (phosphorus)
0
–
0.035
%
S (sulfur)
0
–
0.04
%
Si (silicon)
0.15
–
0.35
%
AISI 51B60 Oil Quenched & Tempered at 650°C Physical properties
Density
7.8
–
7.9
g/cm3
AISI 51B60 Oil Quenched & Tempered at 650°C Mechanical properties
Young’s modulus
201
–
212
GPa
Specific stiffness
25.6
–
27
MN.m/kg
Yield strength (elastic limit)
780
–
960
MPa
Tensile strength
865
–
1070
MPa
Specific strength
99.3
–
122
kN.m/kg
Elongation
16
–
24
% strain
Compressive strength
780
–
960
MPa
Flexural modulus
201
–
212
GPa
Flexural strength (modulus of rupture)
780
–
960
MPa
Shear modulus
77
–
83
GPa
Bulk modulus
155
–
173
GPa
Poisson’s ratio
0.285
–
0.295
Shape factor
28
Hardness – Vickers
265
–
325
HV
Elastic stored energy (springs)
1490
–
2210
kJ/m3
Fatigue strength at 10^7 cycles
386
–
448
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles