AISI 51B60 Oil Quenched & Tempered at 425°C Material Data Sheet
AISI 51B60 Oil Quenched & Tempered at 425°C Material Data Sheet
AISI 51B60 Oil Quenched & Tempered at 425°C Overview
AISI 51B60 tempered 425°C is AISI 51B60 low alloy steel (UNS G51601) in the oil quenched & tempered at 425°C condition. This AISI 51B60 tempered 425°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 51B60 conditions in our AISI 51B60 yield, tensile and hardness comparison. Looking for AISI 51B60 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 51B60 steel parts in-house and inspects them before shipment.
AISI 51B60 Oil Quenched & Tempered at 425°C Designation
AISI 51B60
Condition
Tempered at 425°C & oil quenched
UNS number
G51601
US name
ASTM 51B60, ~ASTM 50B60, ~ASTM 51B60
AISI 51B60 Oil Quenched & Tempered at 425°C Typical uses
General construction, general mechanical engineering, automotive, tools, axles, gears, springs.
AISI 51B60 Oil Quenched & Tempered at 425°C Composition detail
B (boron)
5e-4
–
0.003
%
C (carbon)
0.56
–
0.64
%
Cr (chromium)
0.7
–
0.9
%
Fe (iron)
97
–
97.8
%
Mn (manganese)
0.75
–
1
%
P (phosphorus)
0
–
0.035
%
S (sulfur)
0
–
0.04
%
Si (silicon)
0.15
–
0.35
%
AISI 51B60 Oil Quenched & Tempered at 425°C Physical properties
Density
7.8
–
7.9
g/cm3
AISI 51B60 Oil Quenched & Tempered at 425°C Mechanical properties
Young’s modulus
201
–
212
GPa
Specific stiffness
25.6
–
27
MN.m/kg
Yield strength (elastic limit)
1340
–
1640
MPa
Tensile strength
1470
–
1800
MPa
Specific strength
171
–
209
kN.m/kg
Elongation
9
–
13
% strain
Compressive strength
1340
–
1640
MPa
Flexural modulus
201
–
212
GPa
Flexural strength (modulus of rupture)
1340
–
1640
MPa
Shear modulus
77
–
83
GPa
Bulk modulus
155
–
173
GPa
Poisson’s ratio
0.285
–
0.295
Shape factor
16
Hardness – Vickers
415
–
505
HV
Elastic stored energy (springs)
4380
–
6460
kJ/m3
Fatigue strength at 10^7 cycles
559
–
646
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles