AISI 5160 Oil Quenched & Tempered at 540°C Material Data Sheet
AISI 5160 Oil Quenched & Tempered at 540°C Overview
| AISI 5160 tempered 540°C is AISI 5160 low alloy steel (UNS G51600) in the oil quenched & tempered at 540°C condition. This AISI 5160 tempered 540°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 5160 conditions in our AISI 5160 yield, tensile and hardness comparison. Looking for AISI 5160 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 5160 steel parts in-house and inspects them before shipment. |
AISI 5160 Oil Quenched & Tempered at 540°C Designation
| AISI 5160 | |
| Condition | Tempered at 540°C & oil quenched |
| UNS number | G51600 |
| US name | SAE 5160H, SAE 5160, ASTM G51600, ASTM 5160H, ASTM 5160, ~ASTM 5160 |
| JIS (Japanese) name | SUP9M |
AISI 5160 Oil Quenched & Tempered at 540°C Typical uses
| General construction, general mechanical engineering, automotive, tools, axles, gears, springs. |
AISI 5160 Oil Quenched & Tempered at 540°C Composition detail
| C (carbon) | 0.56 | – | 0.64 | % |
| Cr (chromium) | 0.7 | – | 0.9 | % |
| Fe (iron) | 97 | – | 97.8 | % |
| Mn (manganese) | 0.75 | – | 1 | % |
| P (phosphorus) | 0 | – | 0.035 | % |
| S (sulfur) | 0 | – | 0.04 | % |
| Si (silicon) | 0.15 | – | 0.35 | % |
AISI 5160 Oil Quenched & Tempered at 540°C Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 5160 Oil Quenched & Tempered at 540°C Mechanical properties
| Young’s modulus | 205 | – | 213 | GPa |
| Specific stiffness | 26.1 | – | 27.2 | MN.m/kg |
| Yield strength (elastic limit) | 935 | – | 1150 | MPa |
| Tensile strength | 1050 | – | 1290 | MPa |
| Specific strength | 119 | – | 146 | kN.m/kg |
| Elongation | 9 | – | 15 | % strain |
| Compressive strength | 935 | – | 1150 | MPa |
| Flexural modulus | 205 | – | 213 | GPa |
| Flexural strength (modulus of rupture) | 935 | – | 1150 | MPa |
| Shear modulus | 79 | – | 83 | GPa |
| Bulk modulus | 158 | – | 174 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 23 | |||
| Hardness – Vickers | 305 | – | 375 | HV |
| Elastic stored energy (springs) | 2110 | – | 3110 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 441 | – | 511 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 385 | – | 586 | MPa |
AISI 5160 Oil Quenched & Tempered at 540°C Impact & fracture properties
| Fracture toughness | 39 | – | 67 | MPa.m0.5 |
| Toughness (G) | 7.71 | – | 20.3 | kJ/m2 |
AISI 5160 Oil Quenched & Tempered at 540°C Thermal properties
| Melting point | 1380 | – | 1490 | °C |
| Maximum service temperature | 500 | – | 530 | °C |
| Minimum service temperature | -63 | – | -38 | °C |
| Thermal conductivity | 41 | – | 48 | W/m.°C |
| Specific heat capacity | 440 | – | 520 | J/kg.°C |
| Thermal expansion coefficient | 11.5 | – | 13 | µstrain/°C |
| Thermal shock resistance | 360 | – | 456 | °C |
| Thermal distortion resistance | 3.29 | – | 4 | MW/m |
| Latent heat of fusion | 265 | – | 280 | kJ/kg |
AISI 5160 Oil Quenched & Tempered at 540°C Electrical properties
| Electrical resistivity | 22 | – | 30 | µohm.cm |
| Electrical conductivity | 5.75 | – | 7.84 | %IACS |
| Galvanic potential | -0.5 | – | -0.42 | V |
AISI 5160 Oil Quenched & Tempered at 540°C Magnetic properties
| Magnetic type | Magnetic |
AISI 5160 Oil Quenched & Tempered at 540°C Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5110 | – | 5210 | m/s |
| Mechanical loss coefficient (tan delta) | 3.4e-4 | – | 4.3e-4 | |
AISI 5160 Oil Quenched & Tempered at 540°C Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Excellent |
| Metal hot forming | Excellent |
| Metal press forming | Excellent |
| Metal deep drawing | Limited use |
| Machining speed | 14 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Poor |
| Carbon equivalency | 0.825 – 0.987 |
AISI 5160 Oil Quenched & Tempered at 540°C Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) | Acceptable |
| Flammability | Non-flammable |
AISI 5160 Oil Quenched & Tempered at 540°C Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments | Slightly susceptible |
AISI 5160 Oil Quenched & Tempered at 540°C Standards with similar compositions
| Argentina: IRAM 5160 to IAS |
| Australia: 5160 to AS 1444 |
| Belgium: 55Cr3 to NBN 235-05, 55Cr3 to NBN 253-05 |
| France: 55C3 to AFNOR NF A35-571 |
| Germany: 1.7176 to DIN 17221, 55Cr3 to DIN 17221 |
| Hungary: 60Cr3 to MSZ 2666, 60CrB3 to MSZ 2666 |
| International: 55Cr3 to ISO 683-14, 60Cr3 to ISO 683-14 |
| Italy: 55Cr3 to UNI 3545 |
| Japan: SUP 9 to JIS G4801, SUP 9A to JIS G4801, SUP11A to JIS G4801, SUP9M to JIS G3311 |
| Mexico: 5160 to NMX-B-203-SCFI, 5160 to NMX-B-300, 5160H to NMX-B-268, 5160H to NMX-B-300, 51B60 to NMX-B-203-SCFI, 51B60 to NMX-B-300, 51B60H to NMX-B-268, 51B60H to NMX-B-300 |
| Pan America: 5160 to COPANT 334 |
| Serbia and Montenegro: C.4332 |
| South Korea: SPS 5 to KS D 3701, SPS 5A to KS D 3701, SPS 7 to KS D 3701, SUP 9 M to KS D 3551 |
| Spain: 55Cr3 to UNE 36015, F.1431 to UNE 36015 |
| Sweden: 2253 to SS 142253, 2254 to SS 142254 |
| Turkey: 55Cr3-1 to TS 2288, 55Cr3-1 to TS 7176 |
| UK: 525A58 to BS 970/2, 525A60 to BS 970/2, 525H60 to BS 970/2, 527A60 to BS 970/1, 527A60 to BS 970/5, 527H60 to BS 970/5 |
| USA: 5160, 5160 to ASTM A29/A29M, 5160 to ASTM A331-95, 5160 to ASTM A519, 5160 to ASTM A829/A829M, 5160 to SAE J404, 5160H to ASTM A331-95, 51B60 to ASTM A331-95, 51B60 to ASTM A519, 51B60 to SAE J404, 51B60H to ASTM A331-95, G51600 to ASTM A1031, G51600 to ASTM A506, UNS G51600, UNS G51601, UNS H51600 |
| Tradenames: F 1 KB, KRUPP 55 CR 3, SAARSTAHL 55 CR 3, SHARON 5100 SERIES C, VR-60, XK5160S, ZAPP VC12 |