AISI 5140 Oil Quenched & Tempered at 205°C Material Data Sheet
AISI 5140 Oil Quenched & Tempered at 205°C Overview
| AISI 5140 tempered 205°C is AISI 5140 low alloy steel (UNS G51400, EN 41Cr4) in the oil quenched & tempered at 205°C condition. This AISI 5140 tempered 205°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 5140 conditions in our AISI 5140 yield, tensile and hardness comparison. Looking for AISI 5140 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 5140 steel parts in-house and inspects them before shipment. |
AISI 5140 Oil Quenched & Tempered at 205°C Designation
| AISI 5140 | |
| Condition | Tempered at 205°C & oil quenched |
| UNS number | G51400 |
| US name | SAE 5140, ASTM 5140, ASTM 5140H, ASTM 5140, ~ASTM G51400 |
| EN name | ~41CrS4, ~41Cr4 |
| EN number | ~1.7045, ~1.7039, ~1.7035 |
| ISO name | ~ 41 CrS 4, ~ 41 Cr 4, ~41Cr4 |
| GB (Chinese) name | ~ 40Cr, ~40Cr, ~38CrA |
| JIS (Japanese) name | ~SCr440M |
AISI 5140 Oil Quenched & Tempered at 205°C Typical uses
| General construction, general mechanical engineering, automotive, tools, axles, gears, springs. |
AISI 5140 Oil Quenched & Tempered at 205°C Composition detail
| C (carbon) | 0.38 | – | 0.43 | % |
| Cr (chromium) | 0.7 | – | 0.9 | % |
| Fe (iron) | 97.3 | – | 98.1 | % |
| Mn (manganese) | 0.7 | – | 0.9 | % |
| P (phosphorus) | 0 | – | 0.035 | % |
| S (sulfur) | 0 | – | 0.04 | % |
| Si (silicon) | 0.15 | – | 0.35 | % |
AISI 5140 Oil Quenched & Tempered at 205°C Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 5140 Oil Quenched & Tempered at 205°C Mechanical properties
| Young’s modulus | 209 | – | 217 | GPa |
| Specific stiffness | 26.6 | – | 27.7 | MN.m/kg |
| Yield strength (elastic limit) | 1480 | – | 1810 | MPa |
| Tensile strength | 1610 | – | 1980 | MPa |
| Specific strength | 188 | – | 230 | kN.m/kg |
| Elongation | 7 | – | 11 | % strain |
| Compressive strength | 1480 | – | 1810 | MPa |
| Flexural modulus | 209 | – | 217 | GPa |
| Flexural strength (modulus of rupture) | 1480 | – | 1810 | MPa |
| Shear modulus | 80 | – | 85 | GPa |
| Bulk modulus | 162 | – | 177 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 15 | |||
| Hardness – Vickers | 440 | – | 540 | HV |
| Elastic stored energy (springs) | 5150 | – | 7580 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 597 | – | 690 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 522 | – | 789 | MPa |
AISI 5140 Oil Quenched & Tempered at 205°C Impact & fracture properties
| Fracture toughness | 24 | – | 48 | MPa.m0.5 |
| Toughness (G) | 2.96 | – | 9.89 | kJ/m2 |
AISI 5140 Oil Quenched & Tempered at 205°C Thermal properties
| Melting point | 1430 | – | 1510 | °C |
| Maximum service temperature | 165 | – | 195 | °C |
| Minimum service temperature | -53 | – | -23 | °C |
| Thermal conductivity | 44 | – | 49 | W/m.°C |
| Specific heat capacity | 430 | – | 480 | J/kg.°C |
| Thermal expansion coefficient | 12 | – | 13.5 | µstrain/°C |
| Thermal shock resistance | 536 | – | 676 | °C |
| Thermal distortion resistance | 3.37 | – | 3.95 | MW/m |
| Latent heat of fusion | 265 | – | 280 | kJ/kg |
AISI 5140 Oil Quenched & Tempered at 205°C Electrical properties
| Electrical resistivity | 20 | – | 26 | µohm.cm |
| Electrical conductivity | 6.63 | – | 8.62 | %IACS |
| Galvanic potential | -0.5 | – | -0.42 | V |
AISI 5140 Oil Quenched & Tempered at 205°C Magnetic properties
| Magnetic type | Magnetic |
AISI 5140 Oil Quenched & Tempered at 205°C Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5160 | – | 5260 | m/s |
| Mechanical loss coefficient (tan delta) | 2.2e-4 | – | 2.8e-4 | |
AISI 5140 Oil Quenched & Tempered at 205°C Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Excellent |
| Metal hot forming | Excellent |
| Metal press forming | Excellent |
| Metal deep drawing | Limited use |
| Machining speed | 9.45 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Good |
| Carbon equivalency | 0.637 – 0.76 |
AISI 5140 Oil Quenched & Tempered at 205°C Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) | Acceptable |
| Flammability | Non-flammable |
AISI 5140 Oil Quenched & Tempered at 205°C Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments | Susceptible |
AISI 5140 Oil Quenched & Tempered at 205°C Standards with similar compositions
| Argentina: IRAM 5140 to IAS |
| Australia: 5140 to AS 1440, 5140 to AS 1444, 51B40 to AS 1444, En18 to AS G18, En18D to AS G18 |
| Belgium: 37Cr4 to NBN 251 |
| China: 40Cr to GB/T 11251 |
| Czech Republic: 14140 to CSN 414140 |
| France: 38C4 to AFNOR NF A35-552, 38C4 to AFNOR NF A35-553, 38C4 to AFNOR NF A35-556, 38C4TS to AFNOR NF A35-563, 38Cr4 to AFNOR NF A35-552, 38Cr4 to AFNOR NF A35-553, 38Cr4 to AFNOR NF A35-557, 42C4 to AFNOR NF A35-552, 42C4 to AFNOR NF A35-556, 42C4 to AFNOR NF A35-557, 45C4 to AFNOR NF A35-553, 45C4 to AFNOR NF A35-571 |
| Germany: 1.7035 to DIN 1652, 1.7035 to DIN EN 10083, 41Cr4 to DIN 1652, 41Cr4 to DIN EN 10083 |
| Hungary: Cr3 to MSZ 61, Cr3Z to MSZ 6251 |
| India: 40Cr1 to IS 1570, 40Cr1 to IS 4368, 40Cr4 to IS 11169/1, 40Cr4 to IS 11185, 40Cr4 to IS 13352, 40Cr4 to IS 1570/4, 40Cr4 to IS 3930, 40Cr4 to IS 7494, 40Cr4 to IS 9175/21 |
| International: 3 to ISO 683-7, 37Cr4 to ISO 683-1, 37Cr4 to ISO 683-18, 3a to ISO 683-7, 41Cr4 to ISO 683-1, 41Cr4 to ISO 683-18, 41Cr4E to ISO 4954, 41CrS4 to ISO 683-1, 41CrS4 to ISO 683-18 |
| Italy: 38Cr4 to UNI 8551, 38Cr4KB to UNI 7282, 38Cr4KB to UNI 7356, 41Cr4 to UNI 7874 |
| Japan: SCr4H to JIS G4052 |
| Mexico: 5140 to NMX-B-203-SCFI, 5140 to NMX-B-300, 5140H to NMX-B-268, 5140H to NMX-B-300 |
| Pan America: 5140 to COPANT 334 |
| Romania: 37Cr10 to STAS 11500/2, 40BCr10 to STAS 791, 40Cr10 to STAS 791, 40Cr10S to STAS 791, 40Cr10X to STAS 791, 40Cr10XS to STAS 791 |
| South Korea: SCr 440 H to KS D 3754, SCr 440 to KS D 3707 |
| Spain: 38Cr3 to UNE 36012, 38Cr4 to UNE 36012, 38Cr4DF to UNE 36034, F.1200 to UNE 36012, F.1201 to UNE 36012 |
| Sweden: 2245 to SS 142245 |
| UK: 3/1 to BS 3111/1, 3/2 to BS 3111/1, 41Cr4 to BS EN 10083-1, 41Cr4 to BS EN 10250-3, 41Cr4 to BS EN 10297-1, 50H40 to BS 970/1 |
| USA: 5140 to ASTM A29/A29M, 5140 to ASTM A331-95, 5140 to ASTM A519, 5140 to ASTM A866, 5140 to SAE J404, G51400 to ASTM A1031, G51400 to ASTM A506, UNS G51400, UNS H51400 |
| Tradenames: A-1200, A-1201, A-1202, ALPINE HMV25, ALPINE MAC, BOCHUMER CBVZ, BSO SPEZIAL, CREUSOT 1F3/4, FIRTH-BROWN CCRF, FORTUNA TC4 SPEC, SHARON 5100 SERIES B, TKS 41CR 4, VR-40 |