AISI 50B46 Oil Quenched & Tempered at 650°C Material Data Sheet
AISI 50B46 Oil Quenched & Tempered at 650°C Material Data Sheet
AISI 50B46 Oil Quenched & Tempered at 650°C Overview
AISI 50B46 tempered 650°C is AISI 50B46 low alloy steel (UNS G50461) in the oil quenched & tempered at 650°C condition. This AISI 50B46 tempered 650°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 50B46 conditions in our AISI 50B46 yield, tensile and hardness comparison. Looking for AISI 50B46 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 50B46 steel parts in-house and inspects them before shipment.
AISI 50B46 Oil Quenched & Tempered at 650°C Designation
AISI 50B46
Condition
Tempered at 650°C & oil quenched
UNS number
G50461
US name
ASTM 50B46, ~ASTM 50B44, ~ASME 50B50, ~ASME 50B44
AISI 50B46 Oil Quenched & Tempered at 650°C Typical uses
General construction, general mechanical engineering, automotive, tools, axles, gears, springs.
AISI 50B46 Oil Quenched & Tempered at 650°C Composition detail
B (boron)
5e-4
–
0.003
%
C (carbon)
0.44
–
0.49
%
Cr (chromium)
0.2
–
0.35
%
Fe (iron)
97.7
–
98.5
%
Mn (manganese)
0.75
–
1
%
P (phosphorus)
0
–
0.035
%
S (sulfur)
0
–
0.04
%
Si (silicon)
0.15
–
0.35
%
AISI 50B46 Oil Quenched & Tempered at 650°C Physical properties
Density
7.8
–
7.9
g/cm3
AISI 50B46 Oil Quenched & Tempered at 650°C Mechanical properties
Young’s modulus
201
–
212
GPa
Specific stiffness
25.6
–
27
MN.m/kg
Yield strength (elastic limit)
710
–
875
MPa
Tensile strength
800
–
965
MPa
Specific strength
90.4
–
111
kN.m/kg
Elongation
17
–
27
% strain
Compressive strength
710
–
875
MPa
Flexural modulus
201
–
212
GPa
Flexural strength (modulus of rupture)
710
–
875
MPa
Shear modulus
77
–
83
GPa
Bulk modulus
155
–
173
GPa
Poisson’s ratio
0.285
–
0.295
Shape factor
31
Hardness – Vickers
250
–
305
HV
Elastic stored energy (springs)
1230
–
1840
kJ/m3
Fatigue strength at 10^7 cycles
366
–
418
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
AISI 50B46 Oil Quenched & Tempered at 650°C Thermal properties
Melting point
1420
–
1500
°C
Maximum service temperature
606
–
640
°C
Minimum service temperature
-68
–
-43
°C
Thermal conductivity
40
–
50
W/m.°C
Specific heat capacity
440
–
520
J/kg.°C
Thermal expansion coefficient
11
–
13
µstrain/°C
Thermal shock resistance
279
–
365
°C
Thermal distortion resistance
3.26
–
4.29
MW/m
Latent heat of fusion
265
–
280
kJ/kg
AISI 50B46 Oil Quenched & Tempered at 650°C Electrical properties
Electrical resistivity
15
–
30
µohm.cm
Electrical conductivity
5.75
–
11.5
%IACS
Galvanic potential
-0.51
–
-0.43
V
AISI 50B46 Oil Quenched & Tempered at 650°C Magnetic properties
Magnetic type
Magnetic
AISI 50B46 Oil Quenched & Tempered at 650°C Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5060
–
5200
m/s
Mechanical loss coefficient (tan delta)
4.5e-4
–
5.6e-4
AISI 50B46 Oil Quenched & Tempered at 650°C Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
18.3 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency
0.605 – 0.727
AISI 50B46 Oil Quenched & Tempered at 650°C Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
AISI 50B46 Oil Quenched & Tempered at 650°C Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible
AISI 50B46 Oil Quenched & Tempered at 650°C Standards with similar compositions
France: 38CB1 to AFNOR NF A35-556, 38CBi to AFNOR NF A34-552
Germany: 37CrB1 to DIN
Italy: 38CrB1KB to UNI 7356
Mexico: 50B44 to NMX-B-300, 50B44H to NMX-B-268
Pan America: 50B46 to COPANT 514
USA: 50B44, 50B44 to ASTM A29/A29M, 50B44 to ASTM A519, 50B44 to SAE J770, 50B46, 50B46 to ASTM A322-91, 50B46 to ASTM A752/A752M, 50B46 to SAE J404, 50B46 to SAE J770, UNS G50441, UNS G50461, UNS H50441, UNS H50461