AISI 50B46 Oil Quenched & Tempered at 425°C Material Data Sheet

AISI 50B46 Oil Quenched & Tempered at 425°C Material Data Sheet

AISI 50B46 Oil Quenched & Tempered at 425°C Overview

AISI 50B46 tempered 425°C is AISI 50B46 low alloy steel (UNS G50461) in the oil quenched & tempered at 425°C condition. This AISI 50B46 tempered 425°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 50B46 conditions in our AISI 50B46 yield, tensile and hardness comparison. Looking for AISI 50B46 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 50B46 steel parts in-house and inspects them before shipment.

AISI 50B46 Oil Quenched & Tempered at 425°C Designation

AISI 50B46
ConditionTempered at 425°C & oil quenched
UNS numberG50461
US nameASTM 50B46, ~ASTM 50B44, ~ASME 50B50, ~ASME 50B44

AISI 50B46 Oil Quenched & Tempered at 425°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 50B46 Oil Quenched & Tempered at 425°C Composition detail

B (boron)5e-4–0.003%
C (carbon)0.44–0.49%
Cr (chromium)0.2–0.35%
Fe (iron)97.7–98.5%
Mn (manganese)0.75–1%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 50B46 Oil Quenched & Tempered at 425°C Physical properties

Density7.8–7.9g/cm3

AISI 50B46 Oil Quenched & Tempered at 425°C Mechanical properties

Young’s modulus201–212GPa
Specific stiffness25.6–27MN.m/kg
Yield strength (elastic limit)1120–1380MPa
Tensile strength1250–1540MPa
Specific strength143–175kN.m/kg
Elongation10–16% strain
Compressive strength1120–1380MPa
Flexural modulus201–212GPa
Flexural strength (modulus of rupture)1120–1380MPa
Shear modulus77–83GPa
Bulk modulus155–173GPa
Poisson’s ratio0.285–0.295 
Shape factor19
Hardness – Vickers365–445HV
Elastic stored energy (springs)3060–4540kJ/m3
Fatigue strength at 10^7 cycles500–578MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
436–662MPa

AISI 50B46 Oil Quenched & Tempered at 425°C Impact & fracture properties

Fracture toughness34–61MPa.m0.5
Toughness (G)5.98–16.9kJ/m2

AISI 50B46 Oil Quenched & Tempered at 425°C Thermal properties

Melting point1420–1500°C
Maximum service temperature385–415°C
Minimum service temperature-58–-33°C
Thermal conductivity40–50W/m.°C
Specific heat capacity440–520J/kg.°C
Thermal expansion coefficient11–13µstrain/°C
Thermal shock resistance440–574°C
Thermal distortion resistance3.26–4.29MW/m
Latent heat of fusion265–280kJ/kg

AISI 50B46 Oil Quenched & Tempered at 425°C Electrical properties

Electrical resistivity15–30µohm.cm
Electrical conductivity5.75–11.5%IACS
Galvanic potential-0.51–-0.43V

AISI 50B46 Oil Quenched & Tempered at 425°C Magnetic properties

Magnetic typeMagnetic

AISI 50B46 Oil Quenched & Tempered at 425°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5060–5200m/s
Mechanical loss coefficient (tan delta)2.8e-4–3.6e-4 

AISI 50B46 Oil Quenched & Tempered at 425°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed11.9 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.605 – 0.727

AISI 50B46 Oil Quenched & Tempered at 425°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 50B46 Oil Quenched & Tempered at 425°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Susceptible

AISI 50B46 Oil Quenched & Tempered at 425°C Standards with similar compositions

France: 38CB1 to AFNOR NF A35-556, 38CBi to AFNOR NF A34-552
Germany: 37CrB1 to DIN
Italy: 38CrB1KB to UNI 7356
Mexico: 50B44 to NMX-B-300, 50B44H to NMX-B-268
Pan America: 50B46 to COPANT 514
USA: 50B44, 50B44 to ASTM A29/A29M, 50B44 to ASTM A519, 50B44 to SAE J770, 50B46, 50B46 to ASTM A322-91, 50B46 to ASTM A752/A752M, 50B46 to SAE J404, 50B46 to SAE J770, UNS G50441, UNS G50461, UNS H50441, UNS H50461
Tradenames: KRUPP 37 CRB 1, KRUPP 46 CRB 2