AISI 4620 Annealed Overview

AISI 4620 annealed is AISI 4620 low alloy steel (UNS G46200) in the annealed condition. This AISI 4620 annealed material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 4620 conditions in our AISI 4620 yield, tensile and hardness comparison. Looking for AISI 4620 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 4620 steel parts in-house and inspects them before shipment.

AISI 4620 Annealed Designation

AISI 4620
ConditionAnnealed
UNS numberG46200
US nameSAE 4620, ASTM G46200, ASTM 4621, ASTM 4620, ~SAE 4620H, ~ASTM G46200, ~ASTM 4620

AISI 4620 Annealed Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 4620 Annealed Composition detail

C (carbon)0.17–0.22%
Fe (iron)96.4–97.4%
Mn (manganese)0.45–0.65%
Mo (molybdenum)0.2–0.3%
Ni (nickel)1.65–2%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 4620 Annealed Physical properties

Density7.8–7.9g/cm3

AISI 4620 Annealed Mechanical properties

Young’s modulus201–212GPa
Specific stiffness25.6–27MN.m/kg
Yield strength (elastic limit)330–415MPa
Tensile strength460–560MPa
Specific strength42–52.9kN.m/kg
Elongation24–38% strain
Compressive strength330–415MPa
Flexural modulus201–212GPa
Flexural strength (modulus of rupture)330–415MPa
Shear modulus77–83GPa
Bulk modulus155–173GPa
Poisson’s ratio0.285–0.295 
Shape factor56
Hardness – Vickers140–170HV
Elastic stored energy (springs)267–413kJ/m3
Fatigue strength at 10^7 cycles248–286MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
216–328MPa

AISI 4620 Annealed Impact & fracture properties

Fracture toughness66–106MPa.m0.5
Toughness (G)22.1–52kJ/m2

AISI 4620 Annealed Thermal properties

Melting point1480–1520°C
Maximum service temperature639–661°C
Minimum service temperature-73–-48°C
Thermal conductivity43–49W/m.°C
Specific heat capacity410–460J/kg.°C
Thermal expansion coefficient11–13µstrain/°C
Thermal shock resistance130–173°C
Thermal distortion resistance3.46–4.26MW/m
Latent heat of fusion265–280kJ/kg

AISI 4620 Annealed Electrical properties

Electrical resistivity15–25µohm.cm
Electrical conductivity6.9–11.5%IACS
Galvanic potential-0.51–-0.43V

AISI 4620 Annealed Magnetic properties

Magnetic typeMagnetic

AISI 4620 Annealed Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5060–5200m/s
Mechanical loss coefficient (tan delta)8.7e-4–0.00108 

AISI 4620 Annealed Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed30.5 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.395 – 0.522

AISI 4620 Annealed Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 4620 Annealed Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 4620 Annealed Standards with similar compositions

Australia: 4615 to AS 1444, 4620 to AS 1444, 4620H to AS 1444
France: 20ND8 to AFNOR
India: 20Ni2Mo2 to IS 1570, 20Ni7Mo2 to IS 11169/1, 20Ni7Mo2 to IS 13352, 20Ni7Mo2 to IS 1570/4, 20Ni7Mo2 to IS 5489, 20Ni7Mo2 to IS 9175/31
Mexico: 4615 to NMX-B-203-SCFI, 4615 to NMX-B-300, 4620 to NMX-B-203-SCFI, 4620 to NMX-B-300, 4620H to NMX-B-268, 4620H to NMX-B-300, 4621H to NMX-B-268, 4621H to NMX-B-300
Pan America: 4615 to COPANT 514, 4620 to COPANT 334, 4620 to COPANT 514
Spain: 20NiMo5 to UNE 36027, F.1526 to UNE 36027
UK: 665H17 to BS 970/1, 665H23 to BS 970/1, 665M17 to BS 970/1, 665M20 to BS 970/1, 665M23 to BS 970/1
USA: 4615, 4615 to ASTM A29/A29M, 4615 to ASTM A331-95, 4615 to ASTM A519, 4615 to ASTM A829/A829M, 4615 to SAE J404, 4617, 4617 to ASTM A519, 4617 to ASTM A829/A829M, 4620, 4620 to ASTM A29/A29M, 4620 to ASTM A331-95, 4620 to ASTM A519, 4620 to ASTM A829/A829M, 4620 to FED QQ-S-626C, 4620 to SAE J404, 4620H to ASTM A534, 4621, 4621 to ASTM A29/A29M, 4621 to ASTM A331-95, 4621 to ASTM A519, G46150 to ASTM A1031, G46200 to ASTM A1031, Grade 3 to ASTM A646-95, UNS G46150, UNS G46170, UNS G46200, UNS G46210, UNS H46200, UNS H46210, X4620