How do the AISI 9255 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 9255 (UNS G92550, EN 55Si7) side by side for 7 conditions: Annealed, Normalized, Oil Quenched & Tempered at 205°C, Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 9255 material data sheets linked below.

AISI 9255 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Annealed435–540695–855210–26018–26
Normalized520–640835–1030248–30316–24
Oil Quenched & Tempered at 205°C1840–22601890–2320540–6601–2
Oil Quenched & Tempered at 315°C1610–19801740–2140518–6383–5
Oil Quenched & Tempered at 425°C1340–16401450–1780428–5286–10
Oil Quenched & Tempered at 540°C990–12201130–1380318–39312–18
Oil Quenched & Tempered at 650°C730–895890–1100260–32016–24

AISI 9255 Differences Compared with Annealed

The table below shows how much each condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Normalized+19%+20%+17%-9%
Oil Quenched & Tempered at 205°C+321%+172%+155%-93%
Oil Quenched & Tempered at 315°C+268%+150%+146%-82%
Oil Quenched & Tempered at 425°C+206%+108%+103%-64%
Oil Quenched & Tempered at 540°C+127%+62%+51%-32%
Oil Quenched & Tempered at 650°C+67%+28%+23%-9%

AISI 9255 Strength and Hardness Charts

AISI 9255 Yield strength (MPa)Annealed435–540Normalized520–640Q&T 205°C1840–2260Q&T 315°C1610–1980Q&T 425°C1340–1640Q&T 540°C990–1220Q&T 650°C730–895
AISI 9255 Tensile strength (MPa)Annealed695–855Normalized835–1030Q&T 205°C1890–2320Q&T 315°C1740–2140Q&T 425°C1450–1780Q&T 540°C1130–1380Q&T 650°C890–1100
AISI 9255 Hardness (HV)Annealed210–260Normalized248–303Q&T 205°C540–660Q&T 315°C518–638Q&T 425°C428–528Q&T 540°C318–393Q&T 650°C260–320

AISI 9255 Heat Treatment Key Points

The highest tensile strength is reached in the oil quenched & tempered at 205°C condition (1890–2320 MPa). The softest condition is annealed (210–260 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 205°C to 650°C lowers hardness from 540–660 HV to 260–320 HV, trading strength for toughness and ductility.

AISI 9255 Material Data Sheets

AISI 9255 Annealed | AISI 9255 Normalized | AISI 9255 Oil Quenched & Tempered at 205°C | AISI 9255 Oil Quenched & Tempered at 315°C | AISI 9255 Oil Quenched & Tempered at 425°C | AISI 9255 Oil Quenched & Tempered at 540°C | AISI 9255 Oil Quenched & Tempered at 650°C | All AISI 9255 conditions

Looking for AISI 9255 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 9255 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.