AISI 8640 Tempering Temperature Comparison (315–650°C): Yield, Tensile & Hardness

How do the AISI 8640 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 8640 (UNS G86400) side by side for 4 conditions: Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 8640 material data sheets linked below.

AISI 8640 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Oil Quenched & Tempered at 315°C1360–16701490–1820415–5058–12
Oil Quenched & Tempered at 425°C1170–14301240–1520360–4439–15
Oil Quenched & Tempered at 540°C925–1140990–1220308–37812–20
Oil Quenched & Tempered at 650°C720–880805–990255–31516–24

AISI 8640 Differences Compared with Oil Quenched & Tempered at 315°C

The table below shows how much each condition differs from the oil quenched & tempered at 315°C condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Oil Quenched & Tempered at 425°C-14%-17%-13%+20%
Oil Quenched & Tempered at 540°C-32%-33%-25%+60%
Oil Quenched & Tempered at 650°C-47%-46%-38%+100%

AISI 8640 Strength and Hardness Charts

AISI 8640 Yield strength (MPa)Q&T 315°C1360–1670Q&T 425°C1170–1430Q&T 540°C925–1140Q&T 650°C720–880
AISI 8640 Tensile strength (MPa)Q&T 315°C1490–1820Q&T 425°C1240–1520Q&T 540°C990–1220Q&T 650°C805–990
AISI 8640 Hardness (HV)Q&T 315°C415–505Q&T 425°C360–443Q&T 540°C308–378Q&T 650°C255–315

AISI 8640 Heat Treatment Key Points

The highest tensile strength is reached in the oil quenched & tempered at 315°C condition (1490–1820 MPa). The softest condition is oil quenched & tempered at 650°C (255–315 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 315°C to 650°C lowers hardness from 415–505 HV to 255–315 HV, trading strength for toughness and ductility.

AISI 8640 Material Data Sheets

AISI 8640 Oil Quenched & Tempered at 315°C | AISI 8640 Oil Quenched & Tempered at 425°C | AISI 8640 Oil Quenched & Tempered at 540°C | AISI 8640 Oil Quenched & Tempered at 650°C | All AISI 8640 conditions

Looking for AISI 8640 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 8640 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.