AISI 6150 Annealed vs Normalized vs Quenched & Tempered (205–650°C): Yield, Tensile & Hardness Compared

How do the AISI 6150 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 6150 (UNS G61500, EN 51CrMnV4) side by side for 7 conditions: Annealed, Normalized, Oil Quenched & Tempered at 205°C, Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 6150 material data sheets linked below.

AISI 6150 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Annealed370–455595–740183–22518–28
Normalized550–680845–1040248–30317–27
Oil Quenched & Tempered at 205°C1520–18601740–2130483–5936–10
Oil Quenched & Tempered at 315°C1410–17401550–1900433–5336–10
Oil Quenched & Tempered at 425°C1200–14701290–1590378–4638–12
Oil Quenched & Tempered at 540°C960–11801040–1280310–38010–16
Oil Quenched & Tempered at 650°C755–925850–1040253–31313–21

AISI 6150 Differences Compared with Annealed

The table below shows how much each condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Normalized+49%+41%+35%-4%
Oil Quenched & Tempered at 205°C+310%+190%+164%-65%
Oil Quenched & Tempered at 315°C+282%+158%+137%-65%
Oil Quenched & Tempered at 425°C+224%+116%+106%-57%
Oil Quenched & Tempered at 540°C+159%+74%+69%-43%
Oil Quenched & Tempered at 650°C+104%+42%+39%-26%

AISI 6150 Strength and Hardness Charts

AISI 6150 Yield strength (MPa)Annealed370–455Normalized550–680Q&T 205°C1520–1860Q&T 315°C1410–1740Q&T 425°C1200–1470Q&T 540°C960–1180Q&T 650°C755–925
AISI 6150 Tensile strength (MPa)Annealed595–740Normalized845–1040Q&T 205°C1740–2130Q&T 315°C1550–1900Q&T 425°C1290–1590Q&T 540°C1040–1280Q&T 650°C850–1040
AISI 6150 Hardness (HV)Annealed183–225Normalized248–303Q&T 205°C483–593Q&T 315°C433–533Q&T 425°C378–463Q&T 540°C310–380Q&T 650°C253–313

AISI 6150 Heat Treatment Key Points

The highest tensile strength is reached in the oil quenched & tempered at 205°C condition (1740–2130 MPa). The softest condition is annealed (183–225 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 205°C to 650°C lowers hardness from 483–593 HV to 253–313 HV, trading strength for toughness and ductility.

AISI 6150 Material Data Sheets

AISI 6150 Annealed | AISI 6150 Normalized | AISI 6150 Oil Quenched & Tempered at 205°C | AISI 6150 Oil Quenched & Tempered at 315°C | AISI 6150 Oil Quenched & Tempered at 425°C | AISI 6150 Oil Quenched & Tempered at 540°C | AISI 6150 Oil Quenched & Tempered at 650°C | All AISI 6150 conditions

Looking for AISI 6150 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 6150 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.